◆ Rebuild

Part 14 · Electronics and Computing

Pure Silicon

Silicon is made from quartz and charcoal in an electric arc furnace, then purified in stages — washed in acid, turned into a liquid chloride that can be distilled like spirit, turned back into silicon, and finally zone-refined and grown into a single perfect crystal. Each stage is harder than the last; even the first gives a material that makes excellent radio detectors.

Difficulty
●●●●●
Time
A day per furnace run for crude silicon; weeks to set up chlorination and distillation; months to years for crystal-grade material
Steps from zero
32 prerequisites →

You need first

The Electric Arc FurnaceHydrochloric Acid

This unlocks

Silicones and Synthetic RubbersGermanium, Gallium and Compound SemiconductorsMaking MicrochipsSemiconductors and the Transistor
The full path from nothing — 32 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Bricks
  14. Lime
  15. Salt
  16. Lye and Potash
  17. The Wheel and Axle
  18. Firebrick and Refractories
  19. Glass
  20. Bellows
  21. Saltpeter
  22. Gears
  23. Iron (the Bloomery)
  24. Copper Smelting
  25. Sulfuric Acid
  26. The Waterwheel
  27. Blacksmithing
  28. Hydrochloric Acid
  29. Magnets
  30. Copper Wire
  31. The Generator
  32. The Electric Arc Furnace
  33. Pure Silicon

Do them roughly in this order. See it on the tech tree →

Why it matters

Silicon is the second most common element in the Earth's crust — every grain of sand and every lump of quartz is nearly half silicon by weight — but it never occurs as the element. Freed from oxygen it is a hard, grey, shiny, brittle solid that looks like a metal but conducts electricity only feebly. That feeble conduction, and the way tiny traces of other elements change it, is what makes Semiconductors and the Transistor: diodes, transistors, Solar Cells and Integrated Circuits.

It is also the material that demands the most purity of anything people make. Different uses need very different grades:

Grade Purity Made by Good for
Metallurgical 98–99% Arc furnace Steel and aluminium alloys, chemistry, crystal radio detectors (Radio)
Acid-washed 99.5–99.9% Crushing and leaching Better detectors; starting material for the next step
Chemical (polysilicon) 99.9999% and better Chlorides, distillation, reduction Solar cells, power diodes, first transistors
Electronic (single crystal) 99.9999999% Zone refining or crystal pulling from chemical silicon Transistors and chips

Be honest with yourself about the scale. Metallurgical silicon is within reach of anyone who has built an arc furnace. Each further stage needs more chemistry, more glassware, more power and more care. The last stages were developed by teams of specialists at Bell Laboratories, DuPont, Siemens and Texas Instruments in the 1940s and 1950s, building on everything else in this book. They are described here so that nothing has to be rediscovered — but expect them to take a community, not a person.

How it works

Getting silicon out of quartz

Silicon holds oxygen extremely tightly — far more tightly than iron does. Only carbon at a white heat, above about 1,800 °C, can pull the oxygen away:

quartz (silicon dioxide) + carbon → silicon + carbon monoxide

That temperature is beyond any fuel-fired furnace, so it needs the submerged electric arc (The Electric Arc Furnace). Every impurity in the quartz and in the charcoal ash — iron, aluminium, calcium, titanium — ends up in the silicon.

Three ways to purify

  1. Impurities hide between the grains. As silicon freezes, the impurities are pushed into the last liquid, which freezes as thin films between the crystal grains. Crush the silicon finely and wash it in acid: the films dissolve, the silicon does not.
  2. Turn it into a liquid and distil it. Silicon combines with chlorine to make colourless liquids that boil at low temperatures — silicon tetrachloride (boils at 58 °C) and trichlorosilane (32 °C). They can be distilled like alcohol (Distillation), leaving almost every impurity behind. The pure liquid is then turned back into silicon.
  3. Impurities prefer the liquid. When molten silicon freezes slowly, most impurities stay in the melt rather than join the growing crystal. Move a narrow molten zone slowly along a bar and it sweeps impurities to one end. This is zone refining. Growing a single crystal slowly from a melt has the same effect.

Two impurities matter more than all the rest: boron and phosphorus. Even one atom in a million of either makes pure silicon conduct many thousands of times better. Freezing hardly removes boron at all (see the table under Zone refining), so it must be removed in the chemical stage.

What you need

Item Notes
Submerged-arc furnace The Electric Arc Furnace, with graphite electrodes and a The Generator of tens of kilowatts
Quartz, purest you can find 100 kg per run, in lumps 2–10 cm
Low-ash charcoal 60–70 kg; from clean hardwood, bark removed (Charcoal)
Wood chips 30 kg, to keep the charge open
Hydrochloric acid Strong, several litres per kilogram of silicon (Hydrochloric Acid)
Chlorine or dry hydrogen chloride gas Chlorine and Bleach, Hydrochloric Acid
Hard glass or fused-quartz tubes, flasks, condensers, a fractionating column Laboratory Glassware
Tube furnace to 1,000 °C Charcoal-fired, or wound with resistance wire
Pure zinc, or pure dry hydrogen Zinc and Brass, Hydrogen, Oxygen and Gases
Ice and salt For cooling condensers below 0 °C (Ice and Refrigeration)
For zone refining: a radio-frequency heater of several kilowatts Built from Amplifiers and Oscillators

Where to find it

  • Quartz: the purest is clear or milky-white vein quartz and clean quartzite, without rusty stains or dark specks. Break lumps open; reject any with brown iron stains or glittering mica. Wash, then soak suspect lumps in hydrochloric acid for a day: if the acid turns yellow, there is iron at the surface — wash it off or choose another source. Heating to red and quenching in water cracks it into crushable lumps. White quartz sand from beaches and dunes is often 98–99% silica, but sand is too fine for the furnace except mixed into briquettes.
  • Charcoal: hardwood charcoal holds 1–3% ash (mainly calcium and potassium). Strip bark before charring — bark holds most of the ash.
  • Chlorine: warm strong hydrochloric acid with black manganese ore (pyrolusite) — see Chlorine and Bleach and Hydrochloric Acid. Or electrolyse brine (Electrolysis).
  • Zinc: from sphalerite (Zinc and Brass). Zinc is made by distillation, so it is already fairly pure; distil it again for this use.

Step 1: Metallurgical silicon in the arc furnace

Follow The Electric Arc Furnace for the furnace, electrodes and power. For silicon:

  1. Charge: by weight, quartz 100, charcoal 60–70, wood chips 30. Quartz lumps 2–10 cm; charcoal 1–5 cm.
  2. Run with the electrode buried deep in the charge (submerged arc), feeding fresh charge on top as it sinks. Carbon monoxide burns in blue-yellow flames all over the surface.
  3. Watch the balance. Too little carbon and a sticky, glassy crust of half-reduced silica forms and the furnace "freezes"; too much and the charge conducts too well, the electrode rides up and the heat leaves the bottom. Adjust the next charges.
  4. Tap every 1–2 hours into a mould of graphite or dry sand. The silicon runs out at about 1,500 °C, glowing white-yellow, and freezes into a grey, shining, brittle cake.
  5. Power. A large modern furnace uses about 11–13 kilowatt-hours of electricity for each kilogram; a small one, 15–20 or more. A furnace drawing 50 kW for a day may yield 40–60 kg.

Break the cake with a hammer. Clean silicon is steel-grey with a bright, slightly bluish lustre and breaks with glittering faces. For a radio detector, a chip of this metallurgical silicon touched by a fine brass wire works at once (Radio).

Note Small quantities without an arc furnace. Silica can be reduced by magnesium or aluminium metal powders in a fiercely hot, thermite-like reaction, which chemists used in the nineteenth century. It is violent, needs reactive metal powders you are unlikely to have, and gives a brown, impure powder. This book does not recommend it; the arc furnace is the real route.

Step 2: Acid washing

  1. Crush the silicon in an iron mortar, then grind and sieve to grains under 0.5 mm (fine sand). Pick out any iron scraps from the mortar with a magnet (Magnets).
  2. Leach: cover with hot hydrochloric acid (about 20%, roughly one part strong acid to one of water) in a glass or glazed stoneware vessel, and keep it hot (not boiling) for 6–12 hours, stirring now and then. The acid turns yellow-brown with iron.
  3. Pour off the acid, wash with clean water, and repeat with fresh acid until it stays nearly colourless.
  4. Rinse many times with the cleanest water you have (rain or distilled), and dry.

This gives silicon of roughly 99.5–99.9%. Store it dry in a stoppered glass jar.

Step 3: Making silicon tetrachloride

Quartz+ charcoal arc furnaceover 1,800 °C Crude silicon98–99% radio detectors, alloys crush, wash inhot acid Washed silicon99.5–99.9% dry chlorine300–400 °C Crude chloridefuming liquid distil 2–3 times,keep 57–58 °C cut Pure silicontetrachloride reduce with zincor hydrogen Polysilicon99.9999% solar cells, first transistors zone refine, orpull a crystal Single crystal99.9999999% transistors and chips What each stage removes acid: iron, aluminium, calcium between grains distillation: boron, phosphorus, metals freezing: the last traces of metals
Fig. 1 The road from quartz to crystal. Each stage removes different impurities: the arc furnace makes crude silicon; acid washing removes metals from between the grains; chlorination and distillation make a liquid free of almost everything; reduction turns it back into silicon; zone refining or crystal pulling gives a single, perfect crystal.
  1. The reactor: a hard-glass or fused-quartz tube about 3 cm across and 60 cm long, lying slightly sloped in a tube furnace. Fill the middle 30 cm with acid-washed silicon grains, plugged at each end with glass wool or loose quartz chips.
  2. Dry chlorine. Make chlorine and pass it through two bottles of strong Sulfuric Acid to dry it. Any water ruins the process. Every joint must be tight and every part dry.
  3. Heat the tube to about 300–400 °C (a scrap of lead laid on the tube melts at 327 °C). Pass the chlorine slowly — a few bubbles a second. Silicon burns in chlorine, so once started the reaction keeps the bed hot by itself; reduce the outside heat and keep the bed below a dull red glow.
  4. Condense. The vapour leaving the tube goes through a glass condenser cooled with ice and salt (−10 °C or colder) into a receiving flask, protected from the air by a drying tube. A colourless to yellowish liquid collects that fumes white where it meets air. That is crude silicon tetrachloride. Iron and aluminium chlorides form yellow-brown solid crusts in the cooler part of the tube just after the furnace; scrape them out between runs.
  5. Lead the spent gas outside through a jar of lime water or lye (Lye and Potash) to catch excess chlorine.

The standard industrial route uses dry hydrogen chloride gas instead of chlorine, at about 300 °C, and makes mainly trichlorosilane, which boils at 32 °C and needs colder condensing. The method is the same in principle.

Step 4: Distillation

  1. Use an all-glass still with a fractionating column 60–100 cm tall packed with short pieces of glass tube or glass beads, a thermometer at the top (The Thermometer), and a condenser cooled with ice water (Distillation, Laboratory Glassware). Keep every opening closed with drying tubes: moist air turns the liquid to silica and acid.
  2. Heat the flask gently in warm water — never a flame — to just above 58 °C.
  3. Throw away the first tenth that comes over below 57 °C: it carries boron chloride (which boils at 12 °C) and other light impurities.
  4. Collect the steady fraction that distils at 57–58 °C.
  5. Leave the last fifth in the flask: it holds phosphorus chloride (boils at 76 °C) and heavier impurities.
  6. Distil again — two or three times — keeping only the steady middle cut each time.

Step 5: Back to silicon

Route A: zinc reduction (simpler)

Boil the pure tetrachloride gently so that its vapour flows, together with zinc vapour from a second heated boat of zinc, through a fused-quartz tube held at about 950 °C. Zinc takes the chlorine:

silicon tetrachloride + zinc → silicon + zinc chloride

Silicon grows on the tube walls as grey needles and crusts; the zinc chloride, still a vapour at that heat, passes on and condenses beyond the furnace as a white solid. Afterwards, leach the silicon in hydrochloric acid to remove any zinc, and wash. DuPont made silicon this way in the 1940s for wartime radar detectors and for the first silicon transistors. Its purity depends on the purity of the zinc.

Route B: hydrogen reduction (the Siemens process, the industry standard)

Inside a sealed quartz or steel bell jar, thin rods of silicon are heated by passing electricity straight through them to about 1,100 °C. A mixture of very pure, dry hydrogen and trichlorosilane vapour flows past. Silicon deposits on the rods, which slowly grow thicker — over days — into rods of very pure "polysilicon". Cold silicon conducts too poorly to heat by its own current, so the rods are first warmed from outside. The process is slow, power-hungry, and dangerous (hydrogen with air explodes), but it gives the purest silicon.

Step 6: Zone refining

Holdersgrip the ends Coil movesup 1–5 mma minute RF heater several kW, a fewmillion cycles a second;water-cooled copper coil Unrefined rodimpurities (red) Molten zone 1–2 cm1,414 °C, held in placeby surface tension Refinedcrystalimpuritiesstay in the melt in a vacuum or an unreactive gas impurity along the bar after several passes bottom (start) → top (end) cut off
Fig. 2 Float-zone refining. A silicon rod is held upright by its ends. A water-cooled coil carrying radio-frequency current melts a narrow band of it; surface tension holds the molten zone in place. As the coil moves slowly upward, silicon freezes behind it, purer than before, and the impurities ride along in the molten zone to the top end.

How strongly impurities stay in the liquid is measured by a number for each element: the fraction that goes into the solid. The smaller the number, the better freezing removes it.

Impurity Fraction into the solid Removed by freezing?
Iron 0.000008 Almost completely, in one pass
Copper 0.0004 Very well
Aluminium 0.002 Very well
Phosphorus 0.35 Slowly, over many passes
Boron 0.8 Hardly at all — must go in the chemical stage

The float zone. Molten silicon (it melts at 1,414 °C) attacks every crucible: it dissolves quartz and reacts with graphite. So the bar is held vertically by its two ends and only a narrow band, 1–2 cm tall, is melted — by a radio-frequency induction coil a few turns of copper tube with cooling water running through it, fed with several kilowatts at a few million cycles a second from a large tube oscillator (Amplifiers and Oscillators). The coil travels slowly along the bar, 1–5 mm a minute, in a vacuum or an unreactive gas. Each pass sweeps impurities towards one end; after several passes, cut that end off. A seed crystal at the start makes the whole bar freeze as a single crystal.

Germanium is easier. It melts at only 938 °C and can be zone-refined lying in a graphite boat inside a glass tube, with a ring-shaped heater pulled slowly along. The first transistors (1947) were germanium for exactly this reason. But germanium is rare: it is recovered in small amounts from the dust and residues of zinc smelting and from some coal ashes (Germanium, Gallium and Compound Semiconductors).

Step 7: Growing a crystal (in outline)

A transistor needs one continuous crystal with all its atoms in line. The Czochralski method: melt pure silicon in a fused-quartz crucible inside a heater, in vacuum or an unreactive gas. Dip in a small seed crystal on a rod, let it start to melt, then pull it up very slowly — about 1–2 mm a minute — while turning it 10–20 times a minute. Silicon freezes onto the seed, copying its arrangement, and a round single crystal grows downward. First pull a thin neck a few millimetres across, which lets flaws grow out, then widen to full size. Traces of boron or phosphorus added to the melt make p-type or n-type crystal; see Semiconductors and the Transistor. From here on, dust, sweat and skin oil are impurities too, so the crystal is cut, polished and worked in a clean room (Making Microchips).

How to tell it worked

  • Metallurgical silicon: grey, metallic, brittle, glittering on fresh breaks. It feels light for a metal (2.3 times water, against iron's 7.9). It is not attracted to a magnet and does not fizz in hydrochloric acid — iron and aluminium would.
  • Acid washing: fresh acid on the washed grains stays clear.
  • It is a semiconductor. Press a piece between two copper clips in a circuit with a cell and a galvanometer (Measuring Electricity). Warm it with a candle flame: the current rises as it warms (a metal would carry less). The purer the silicon, the higher its resistance when cold. A cube 1 cm on a side of very pure silicon has about 2,000 ohms or more; metallurgical silicon, well under one ohm.
  • The hot-probe test. Touch the silicon with two copper points connected to a galvanometer, one point heated in a flame. The needle swings one way for n-type, the other for p-type. Calibrate with a sample of known type once you have one.
  • Tetrachloride: colourless, fumes in air, boils steadily at 57–58 °C. A drop on a clean glass plate evaporates leaving almost no residue.
  • Single crystal: a polished, lightly etched surface looks uniform, with no grain boundaries; a broken piece splits along flat faces.

Note Troubleshooting. Furnace gives slag and no silicon → too little carbon, or the arc is near the surface; more charcoal, electrode deeper, more power. Silicon very full of iron → iron-stained quartz or iron scraps in the charge; choose cleaner quartz, keep iron tools out. Chlorination stops → the bed is coated with silica because of moisture; dry everything again and replace the bed. Distillate turns cloudy and white → moist air getting in; check drying tubes and joints. Zone keeps collapsing in float-zone refining → zone too long; reduce the power or narrow the coil. Crystal grows as many grains → pulled too fast, or the melt temperature is unsteady.

Dangers

Danger Chlorine and chlorosilanes. Chlorine gas destroys the lungs; a few breaths of strong gas can kill. Silicon tetrachloride and trichlorosilane fume violently in moist air, releasing hydrochloric acid gas, and splashes burn skin and eyes. Trichlorosilane is also highly flammable and its vapour can ignite easily. Work outdoors or under a strong draught, with a wet cloth over nose and mouth as the barest protection, eyes shielded, and a bucket of dry sand (not water) for spills. See Chlorine and Bleach and Hydrochloric Acid.

Danger Hydrogen explodes. Hydrogen mixed with air in almost any proportion explodes from a spark. In the Siemens process, flush all air out with an unreactive gas before admitting hydrogen, burn the exhaust at a safe distance, and never open a hot reactor. Some by-products of reducing chlorosilanes with hydrogen catch fire by themselves in air. See Hydrogen, Oxygen and Gases.

Danger The arc furnace gives off carbon monoxide, a fine silica smoke that scars the lungs, ultraviolet light that burns eyes and skin, and molten silicon at 1,500 °C that explodes on contact with water. Follow every warning in The Electric Arc Furnace.

  • Silica dust from crushing quartz causes silicosis, an incurable scarring of the lungs. Crush wet, work in moving air, cover nose and mouth.
  • Hydrochloric acid burns; mix acid into water, not water into acid.
  • Never use hydrofluoric acid, which the modern industry uses to etch silicon. It passes through skin painlessly and destroys bone and heart muscle hours later; small splashes have killed.
  • Radio-frequency heaters carry thousands of volts and burn deeply. See Amplifiers and Oscillators.

What this unlocks

How it was first done

Jöns Jacob Berzelius in Stockholm first isolated silicon in 1823–1824 as a brown powder, by heating potassium with a silicon fluoride compound. Henri Sainte-Claire Deville made crystalline silicon in the 1850s. Electric arc furnaces made ferrosilicon and silicon carbide on an industrial scale from the 1890s, and silicon metal soon after. In 1906 Greenleaf Whittier Pickard patented the silicon crystal detector for radio. During the Second World War, the need for radar detectors drove a search for purer silicon: at Bell Laboratories, Russell Ohl, Jack Scaff and Henry Theuerer found in 1940 that some silicon rods had a boundary inside them that produced a voltage in light — the first p-n junction — and DuPont developed zinc reduction of silicon tetrachloride. William Pfann at Bell Laboratories invented zone refining in 1951, Gordon Teal and John Little grew single crystals of germanium and then silicon by the Czochralski method (named after Jan Czochralski, who discovered crystal pulling with metals in 1916), and Henry Theuerer and others developed float-zone silicon in the early 1950s. In 1954 Teal, by then at Texas Instruments, made the first commercial silicon transistor, and Bell Laboratories made the first practical silicon solar cell. The Siemens hydrogen-reduction process, developed in Germany in the 1950s, still makes most of the world's pure silicon.

Source: content/entries/electronics/pure-silicon.md