◆ Rebuild

Part 15 · Knowledge and Science

Engraving, Seals and Etching

Cutting fine lines into metal with a hardened steel graver — lettering and pictures on tools, plates and instruments, seals and signet rings cut in reverse, and copperplates engraved or etched with acid and printed under a rolling press. Includes making and sharpening gravers, the engraver's ball and sandbag, and the loupe.

Difficulty
●●●●●
Time
An afternoon to make and sharpen a set of gravers; weeks of practice for clean lettering; days to months for an engraved plate
Steps from zero
18 prerequisites →

You need first

SteelPrinting

This unlocks

—
The full path from nothing — 18 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Lye and Potash
  12. Ink
  13. Bellows
  14. Paper
  15. Iron (the Bloomery)
  16. Printing
  17. Blacksmithing
  18. Steel
  19. Engraving, Seals and Etching

Do them roughly in this order. See it on the tech tree →

Why it matters

A steel graver pushed by hand cuts a line in brass or copper finer than a hair that lasts for centuries. With it you can:

  • mark things permanently — names on tools and trophies, numbers on measures and weights, scales on instruments (Scientific Instrument Making), dials on clocks;
  • cut seals — a design sunk in reverse in metal or stone, pressed into wax or clay to prove that a letter, a jar or a document is genuine (Money, Trade and Record-keeping, Organising a Community);
  • make printing plates — copper engraved or etched with lines that hold ink, printed under great pressure. Before photography, every detailed map (Maps and Mapmaking), scientific drawing, banknote, sheet of music and portrait in a book was printed this way.

Letterpress (Printing) prints from raised surfaces. Engraving and etching print from sunken lines — intaglio (Italian for "cut into") — far finer than any woodcut can hold.

How it works

A graver (also called a burin) is a short bar of glass-hard Steel with its end ground at an angle to make a sharp point. Pushed along a softer metal at a low angle, the point ploughs out a curl of metal and leaves a clean groove. A square graver tipped onto its corner cuts a V-shaped groove with a 90° bottom, so the line is twice as wide as it is deep: press the point deeper and the line swells; lift it and the line tapers to nothing. That swelling and tapering is what makes engraved lettering and pictures look alive.

In printing, the plate is covered with stiff ink, then wiped clean so ink stays only in the grooves. Damp paper pressed onto it with heavy pressure is forced into the grooves and lifts the ink out. Deep, wide lines print black; shallow, thin ones print grey. Tone comes from how close the lines are and how they cross.

Etching makes sunken lines with acid instead of muscle: a needle draws through an acid-proof ground and acid eats the exposed lines. It is easier to learn — drawing, not cutting — but less crisp.

What you need

Item Size Notes
Gravers Bars 2.5–3 mm square, 10–12 cm long Square, lozenge, flat, round and knife; high-carbon steel
Handles Mushroom shape, 3 cm across, flat on one side Boxwood or other close-grained hardwood
Oilstones Fine and very fine (novaculite or slate) Sharpening and Honing
Scraper Three-sided steel blade 10 cm long, hollow-ground faces Removes burrs and mistakes
Burnisher Polished hardened steel tongue, 8–10 cm Smooths and closes up scratches
Engraver's ball or sandbag Ball 10–15 cm across; bag 15–20 cm Holds the work, lets it turn
Loupe 3–6 times Lenses
Copper plate 1–1.5 mm thick Copper Smelting, Sheet Metal and Rolling
For etching Ground of wax and resin; steel needles; acid tray Nitric Acid or iron chloride
For printing Rolling press, felt blankets, stiff plate ink, damp paper Below

Where to find it

  • Steel for gravers, scrapers and burnishers: about 1–1.2 % carbon (Steel); old files, softened, reshaped and re-hardened, are ideal.
  • Copper for plates: refined, soft, without pits (Copper Smelting). Brass suits nameplates and seals; zinc etches well but wears quickly in printing.
  • Boxwood for handles, or hawthorn, pear or holly.
  • Polishing: pumice, fine charcoal of willow or lime, rouge from hematite (Abrasives and Grinding Stones).
  • Ground and ink: beeswax (Beekeeping), pine resin and asphalt or pitch (Tar, Pitch and Glue); linseed oil boiled thick (Oils and Pressing) and lampblack (Ink).
  • Sand and leather for the sandbag (Hides and Leather).

Gravers and how to sharpen them

THE SQUARE GRAVER (SIDE VIEW, ENLARGED) CUTTING ENDS THE CUT Handle boxwood, flat underneath Belly 2.5–3 mm square bar, 10–12 cm Face ground and polished at 45° Heel 10–15°, 1–2 mm long (drawn larger) Point Square general Lozenge fine lines Flat clearing Round broad lines Knife hair lines width depth 90° V-groove width = 2 × depth: press deeper and the line swells
Fig. 1 The square graver. The face is ground at 45° to make the point; a short heel ground under the point lets you hold the tool low. Below, the cutting ends of the common shapes, and the V-groove a square graver cuts: twice as wide as it is deep.

Making a graver

  1. Forge or file the bar to 2.5–3 mm square and 10–12 cm long, with a tang 2.5 cm long at one end, bent up about 10° near the handle so your knuckles clear the work.
  2. Shape the section. Square for general cutting; lozenge (diamond-shaped, narrower than it is deep) for fine lines; flat and round (called scorpers) for clearing backgrounds and cutting broad lines; knife (onglette) for very thin lines and fine shading.
  3. Harden. Heat the last 3 cm to a dull cherry red and quench in water. Polish one face and temper by holding the shank over a flame until pale straw (about 220 °C) creeps to the point, then quench (Steel). The point must be file-hard: too soft and it rolls over on brass.
  4. Handle. Turn a mushroom-shaped boxwood handle 3 cm across (Wood Turning and Treen), saw a flat on one side so it can lie low on the plate, and drive the tang in. Fit the length to your hand: with the handle in your palm, the point should reach just past the tip of your outstretched thumb.

Sharpening

  1. The face. Hold the graver at 45° to a fine oilstone, with the face flat on the stone, and rub in small circles until the face is one flat, shining plane meeting the edges in a sharp point. A sharpening jig — a block with a hole drilled at 45° that the graver slides through — makes the angle exact (Sharpening and Honing).
  2. The heel. Lay the belly (the bottom edge behind the point) on the stone and raise the handle 10–15°. Rub a tiny flat 1–2 mm long just behind the point. This heel lets the graver cut at a low angle without the shank dragging.
  3. Polish the face and heel on the finest stone, then on hard leather with rouge. A polished face leaves a bright, shining cut.
  4. The thumbnail test. Rest the point lightly on your thumbnail at a low angle and push gently. A sharp graver catches and sticks; a dull one slides. Re-polish the face as soon as it slides — usually every few minutes of cutting.

Scraper and burnisher

A scraper is a three-sided steel blade 10 cm long, each face hollow-ground so the three edges are keen; it shaves off burrs and scrapes out mistakes. A burnisher is a hardened steel tongue 8–10 cm long, slightly curved, polished like a mirror (on the finest stones and strop); rubbed with oil over a scratch or an unwanted line, it pushes the metal flat and closes it up.

Holding the work

ENGRAVER'S BALL SANDBAG LOUPE Work a seal blank Jaws closed by a screw Leather ring stuffed with sand Iron ball 10–15 cm, 4–8 kg Copper plate turned into the cut Leather bag 15–20 cm, fine sand Lens focus 4–8 cm, 2.5 cm across Horn cup held in the eye magnifies 25 ÷ focus (cm): a 5 cm lens gives 5 times
Fig. 2 Holding the work. The engraver's ball rests on a leather ring and turns and tilts freely, carrying the work in its jaws. A flat plate lies on a sandbag and is turned with the free hand. A loupe in a horn cup magnifies the cut.

Engraving block (engraver's ball)

The cutting hand pushes straight; the work turns to make curves. The engraver's ball holds small objects — rings, seals, nameplates, tool parts — and turns and tilts freely under the other hand.

  1. Cast the ball: a hemisphere of iron or bronze 10–15 cm across, 4–8 kg, with its flat side up (Metal Casting). Weight is what keeps it from skidding.
  2. Jaws: two iron jaws on top, closed by a screw across them (Screws, Nuts and Bolts), with holes for pegs so irregular pieces can be wedged. Line the jaws with leather or lead to protect finished work. Small pieces can be set in a bed of warm shellac or pitch on a wooden block clamped in the jaws.
  3. Ring: sit it on a thick ring of leather stuffed with sand, or a wooden ring with a leather lining, 8–10 cm across. The ball rolls in any direction yet stays put.

A good block sits heavy and turns with one finger; a light one moves under the graver.

Sandbag

For flat plates, sew a round leather cushion 15–20 cm across and fill it tight with fine dry sand. Lay the plate on it; the left hand turns the plate against the graver.

Loupe

A short-focus magnifier. A convex lens of focal length 4–8 cm magnifies about 25 ÷ focal length in cm times: a 5 cm lens gives 5 times. Grind it about 2.5 cm across (Lenses) and mount it in a short horn or wooden cup held in the eye socket like a watchmaker's glass, or on a stand over the work. A good loupe is sharp to the edges of the field, without colour fringes.

Cutting lines and lettering

  1. Prepare. File, stone and polish the metal flat; rub on a film of beeswax or chalk-and-gum to draw on.
  2. Lay out. Rule guidelines with dividers and a scriber for the top and bottom of the letters. Draw the letters lightly in pencil or scratch them faintly with a fine point. For anything that will be printed or pressed — seals and plates — draw it in reverse; check it in a mirror.
  3. Hold the graver with the handle in your palm, the forefinger on top, and the thumb against the side of the shank, its tip resting on the work to steady and brake the cut.
  4. Enter at a steeper angle, about 30°, to start the cut, then lower the handle to 10–15° and push steadily. To end a line, lift the handle a little so the point rises out, and flick out the chip.
  5. Curves: keep the graver hand still and turn the work into the cut with the other hand.
  6. Thick and thin: press deeper or roll the graver slightly onto one side to swell the line; lift to taper.
  7. Clean up burrs with the scraper held nearly flat, and rub lightly with charcoal and water.
  8. Fill lettering on bright metal with black wax or pitch rubbed in warm and scraped off the surface, so it reads at a glance.

Practise on scrap brass: straight lines, curves, then the alphabet. A good line is clean-sided and bright, without stutter marks; slips across the work are the commonest fault and are burnished out.

Seals

1 SEAL FACE 2 PRESSED AND LIFTED 3 THE IMPRESSION R Cut in reverse dark = sunk 0.5–1 mm walls slope outward Wax design stands up Seal R Reads the right way raised, crisp, lifts clean
Fig. 3 An intaglio seal is cut in reverse and sunk into the metal; pressed into warm wax it leaves the design raised and reading the right way. The walls slope outward slightly so the seal lifts clean.

An intaglio seal has its design cut sunken and backwards, so that when pressed into wax, clay or paper it leaves a raised, right-reading impression. Seals sign documents, close letters and stamp goods; a community's official seal is part of how trust works (Organising a Community).

  1. The blank. A brass or bronze disc or oval 15–25 mm across and 5–8 mm thick on a handle or loop, cast or cut from bar. File the face dead flat, stone it, and polish it. For signet rings see Jewellery, Beads and Medals.
  2. The design. Draw it the size of the seal on thin paper, then trace it onto the face reversed. Simple, bold designs work best: initials, a mark, a border with letters round it.
  3. Outline. Cut every outline with a lozenge graver.
  4. Sink the fields. Remove the metal inside the outlines with flat and round scorpers, working down in layers to 0.5–1 mm for letters and up to 1.5 mm for the deepest parts of a picture. Keep the walls sloping outward slightly — never undercut — so the wax releases.
  5. Prove it often. Press it into warm wax, soft clay or bread dough as you go, and read the proof. Correct and deepen.
  6. Polish the sunken parts lightly with a stick and rouge; a smooth intaglio gives a glossy impression.

Steel seals and dies for embossing paper, marking metal or striking coins are cut the same way in annealed steel and then hardened; see Presses, Punches and Dies.

Stone seals. Soft stones (soapstone, serpentine) cut with steel gravers. Hard stones such as agate and carnelian cannot be scratched by steel: they are ground with small iron or copper wheels and drills spun on a bow lathe and charged with emery and oil, the same way as Gem Cutting and Lapidary work. A stone seal never wears.

Copperplate engraving

A copperplate is a sheet of polished copper engraved with a picture or text for intaglio printing.

  1. The plate. Hammer and roll copper to 1–1.5 mm thick (Sheet Metal and Rolling) and cut it 2–3 cm larger all round than the picture. Planish it flat on a smooth anvil with a polished hammer.
  2. Polish with pumice and water, a fine stone, then a block of fine willow charcoal and water, until no scratch shows under the loupe; finish with the burnisher and oil. Every scratch left will print.
  3. Bevel the edges to 45° and round the corners, or they cut paper and blankets.
  4. Transfer the drawing in reverse: lay it face down on a thin film of white wax on the plate and rub the back so the pencil offsets onto the wax. Scratch the lines lightly into the copper.
  5. Engrave: outlines first, then shading. Tone is built from parallel lines, then crossed lines, with dots ("flick" or stipple) in the lightest places. Lines must swell and taper smoothly. Scrape every burr away flush.
  6. Proof it (below) and deepen or add lines. To remove a line, scrape and burnish it away, then tap the hollow level from the back with a small hammer on a smooth anvil.

Two quicker kinds of intaglio:

  • Drypoint. Scratch straight into the copper with a hardened steel needle. The furrow of metal thrown up beside the line (the burr) holds ink and prints a soft, velvety black — but it wears flat after 20–50 prints.
  • Mezzotint. Roughen the whole plate evenly with a rocker — a curved blade with fine teeth — rocked across it in many directions until it prints solid black. Then scrape and burnish away the roughness where you want lighter tones. It gives smooth gradations from black to white, good for portraits.

Etched plates

The ground, needling and biting of a copper etching plate with dilute nitric acid are described in Nitric Acid. Additions:

  • Iron chloride — rust or iron filings dissolved in Hydrochloric Acid and left in air until brown — etches copper without poisonous fumes and is far safer. Hang the plate face down just under the surface, so the sludge falls away. Fine lines take roughly 15–30 minutes, deep ones an hour or more; bite a scrap strip first and time it.
  • Hard ground (2 parts beeswax, 2 parts asphalt or pitch, 1 part rosin) takes needle lines. Soft ground — the same with about a third more tallow — never fully hardens: lay paper over it and draw with a pencil, and the ground lifts where you pressed, giving soft, grainy lines like crayon.
  • Aquatint for tone. Shake fine powdered rosin over the bare plate from a bag of fine cloth or a dust box until it is evenly freckled, then warm the plate from below until the grains just turn clear and stick. Acid bites the spaces between them, giving an even grain that prints as grey. Paint acid-proof varnish over areas that are finished (stopping out) and bite again for darker tones: 1–2 minutes for a pale tint, 10–20 for near-black.
  • Steel plates and blades are etched for marking and decoration in much weaker acid (see Nitric Acid).

Printing intaglio: the copperplate press

ROLLING PRESS (SIDE) INSIDE THE NIP layers drawn apart Pressure screw Star wheel about 1 m Rollers 15–25 cm, hard wood Bed 3–4 cm Plate, paper and felt blankets bed moves Roller Felt blankets Damp paper Ink only in the lines Copper plate surface wiped clean
Fig. 4 The copperplate press and what happens inside it. Turning the star wheel draws the bed, carrying plate, damp paper and felt blankets, between two heavy rollers. The blankets force the paper down into the inked lines.

Intaglio needs far more pressure than letterpress, applied a strip at a time by a rolling press.

Building the press

  1. Frame: two upright cheeks of oak 10–15 cm thick, about 1 m tall, joined by cross-pieces (Doors, Windows and Joinery), on a sturdy base.
  2. Rollers: two cylinders of very hard, close-grained wood (hornbeam, beech, lignum vitae) 15–25 cm across, or cast iron, turned perfectly round and parallel (The Lathe), with iron journals running in bearings in the cheeks (Bearings and Lubrication). The bottom roller is fixed; the top one sits in slots.
  3. Pressure: screws or folded paper and wooden packing above the top roller's bearings press it down. Adjust both sides equally.
  4. Bed: a planed hardwood plank or iron plate 3–4 cm thick and as wide as the rollers, running between them. It must be flat.
  5. Drive: a star wheel of four to six spokes, about 1 m across, fixed to the top roller; or a crank with a pair of gears (Gears) for more force.
  6. Blankets: two or three layers of thick woollen felt (Felt), cut a little smaller than the bed.

Test a press by running an un-inked plate with damp paper: the embossed edge (the plate mark) should be equally deep on all four sides.

Inking and printing

  1. Plate ink: linseed oil heated slowly until it thickens to a syrup ("plate oil", Ink), ground stiff with lampblack or another pigment (Pigments, Paints and Varnish) on a stone slab with a muller. It should be as stiff as soft butter.
  2. Paper: soak strong rag Paper in water for 10–30 minutes and blot it between dry sheets until it is limp and damp but shows no shine of water.
  3. Ink the plate warm — on an iron plate over a gentle fire, about blood heat to hand-hot — dabbing ink into every line with a pad of rolled felt or leather.
  4. Wipe: first with a pad of stiff, starched open-weave cloth in circles, until the lines stand out against a grey film; then with the flat palm of the hand, lightly dusted with chalk, until the surface is clean and bright and only the lines are full.
  5. Print: lay the plate face up on the bed, the paper over it, then the blankets. Turn the star wheel steadily to draw the whole bed through the rollers, without stopping. Lift the blankets and peel the paper off.
  6. Dry the prints flat between blotters under boards.

A copper engraving prints a few hundred to a couple of thousand good impressions before the finest lines wear; a thin coat of iron or nickel plated onto it (Electroplating) adds thousands more and can be renewed. Steel plates, engraved soft and then hardened, print tens of thousands — the way banknotes and stamps were made (Envelopes, Stamps, Clips and Office Supplies).

Wood engraving

A different branch: boxwood end grain, glued up into blocks exactly the height of type, is engraved with gravers and printed with the text in an ordinary Printing press. The cut lines print white and the surface black — the reverse of copperplate.

How to tell it worked

  • Graver: catches on the thumbnail; leaves a bright, clean groove; no ragged edges under the loupe.
  • Lettering: even height and spacing, smooth swells, no slips; reads well after filling.
  • Seal: crisp, right-reading wax impression that lifts out clean.
  • Plate: a proof with rich, even blacks in the lines and clean whites between; plate mark even on all sides.

Note Troubleshooting. Graver slips out of the cut → point dull or face rounded; repolish. Or the handle held too low at the start; enter steeper. Graver digs in and stops → handle too high; lower it. Or the metal is hard; anneal brass and copper by heating to dull red and quenching. Print grey and weak → lines too shallow, ink too thin, paper too dry, or too little pressure. Grey haze over the whole print → plate not wiped clean, or scratches in the polish. Seal tears the wax → undercut walls or a rough intaglio; slope the walls and polish; dust the seal with talc or wet it. Etched lines ragged or "foul biting" in blotches → ground too thin or scratched; acid too strong or bubbles left on the lines.

Dangers

Warning Acids and their fumes. Nitric acid gives off red-brown fumes that injure the lungs hours later; work outdoors and see Nitric Acid. Iron chloride is milder but stains and burns skin and eyes. Always add acid to water, never water to acid, and wear eye protection and an apron.

  • Gravers slip. A graver skidding off the work goes straight into the hand that steadies it. Keep that hand behind or beside the cut, never in front of the point. Keep a cork on each point when not in use.
  • Rosin dust and melted grounds are flammable; shake rosin in a closed box, melt grounds in a water bath, away from flame.
  • Eyes. Hours at a loupe strain the eyes; work in daylight and look far away often.
  • Presses trap fingers between bed and rollers; keep hands off the bed while turning.

What this unlocks

Engraving gives you permanent marks, proof of authenticity, and the printing of anything letterpress cannot: maps (Maps and Mapmaking), plans and technical drawings, scientific illustration, music, banknotes and stamps (Money, Trade and Record-keeping, The Post), and the fine scales of instruments (Scientific Instrument Making). The same skills of ground, acid and resist lead to Blueprints and Cyanotypes, photo-engraving and the printed circuit boards of Building Circuits: Boards, Connectors and Cables.

How it was first done

Engraved seals are older than writing. Stamp seals were pressed into clay in the Near East by about 6000 BC and the rolled cylinder seal appeared in Mesopotamia about 3500 BC; Greeks and Romans cut gems in reverse for signet rings with bow-driven drills and emery. The first engraved prints on paper were made in Germany in the 1430s, probably by goldsmiths, and Martin Schongauer and Albrecht Dürer made copperplate engraving a great art around 1500. Etching came from armourers who decorated steel with acid; Daniel Hopfer of Augsburg etched prints from iron plates about 1500, and Rembrandt made etching famous in the 1600s. Mezzotint was invented by Ludwig von Siegen in 1642, and aquatint was perfected in the 1760s. In England Thomas Bewick made boxwood end-grain engraving the standard way to illustrate books around 1800, and from about 1820 hardened steel plates, developed for banknotes by the American Jacob Perkins, printed the first postage stamps and millions of book illustrations.

Source: content/entries/knowledge/engraving.md