◆ Rebuild

Part 3 · Metals

Soldering and Brazing

Join metal to metal with a second, lower-melting metal that flows into the joint like glue. Soft solder (tin, or tin and lead) seals cans, roofs, pipes and electrical wires; brazing with brass or copper makes joints in iron and steel almost as strong as the metal itself.

Difficulty
●●●●●
Time
An hour to make a soldering iron; minutes per joint once you have the knack
Steps from zero
14 prerequisites →

You need first

Tin and PewterLeadCopper Smelting

This unlocks

Building Circuits: Boards, Connectors and CablesTins, Cans, Drums and Tanks

Objects made here

soldering ironsolder
The full path from nothing — 14 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Bellows
  12. Tin and Pewter
  13. Lead
  14. Copper Smelting
  15. Soldering and Brazing

Do them roughly in this order. See it on the tech tree →

Why it matters

Forge welding joins iron to iron, but only at white heat, only for iron and steel, and only where you can swing a hammer. Rivets join anything but leak and need holes. Soldering joins thin, delicate or awkward pieces at a gentle heat, and makes joints that are watertight and airtight. Brazing does the same at a red heat, with joints strong enough for tools, frames and pressure fittings.

With soft solder you can seal Sheet Metal and Rolling buckets, tinplate cans for Canning and Bottling, lamps, funnels and kettles; join lead and copper water pipes (Pipes, Plumbing and Aqueducts); and — most importantly for later — make reliable electrical joints in Copper Wire, for the The Battery, The Telegraph, Radio and every circuit after. With brazing you can join steel to iron, repair a cracked casting, fix the steel teeth of a band saw or the parts of a The Bicycle, and attach fittings to a The Steam Engine boiler.

How it works

A solder is a metal or alloy that melts at a lower temperature than the metals being joined. Heated together with them, molten solder wets clean metal — it spreads out in a thin film and dissolves a very thin skin of the surface, forming a true metallic bond. It is then drawn into narrow gaps by capillary action, the same force that pulls water up a thin straw or into a cloth. When it freezes, the joint is solid metal all the way through.

Three things must all be right:

  1. Clean metal. Solder will not stick to rust, scale, grease or tarnish. Every surface must be scraped, filed or sanded bright just before joining.
  2. Flux — a substance that dissolves the thin film of oxide that forms on hot metal, and keeps air off while you work.
  3. Both pieces hot. The work itself must be hot enough to melt the solder. Solder dropped onto cold metal just balls up and falls off.

The gap matters too. Capillary action works best in a gap of about 0.05–0.2 mm — a close slide fit. Too wide, and solder will not fill it; pressed tight with no gap at all, it cannot get in.

Soft soldering uses alloys melting below about 450 °C. It is easy, but the joint is weak — perhaps a tenth as strong as iron — so the pieces must be held together mechanically (by folding, lapping, twisting or riveting) and the solder only seals and stiffens. Brazing (also called hard soldering) uses alloys of copper, zinc and silver melting above 450 °C, usually 700–1,100 °C. A good brazed joint with a close gap can be nearly as strong as mild steel.

What you need

Solders

Solder Composition by weight Melts at Use
Fine solder 63 tin : 37 lead (or 60 : 40) 183 °C, all at once Electrical work, fine joints
Tinsmith's solder 50 tin : 50 lead 183–215 °C Tinplate, sheet, general
Plumber's solder 1 tin : 2 lead 183–about 255 °C; pasty in between Wiped joints in lead pipe
Pure tin tin 232 °C Food and drinking-water vessels: no lead
Tin-copper 99 tin : 1 copper about 227 °C Lead-free pipes and wiring
Silver solder about 2 silver : 1 brass 700–780 °C Jewellery, instruments, fine strong joints
Spelter (brazing brass) 1 copper : 1 zinc about 870–880 °C Brazing iron, steel, copper
Copper pure copper 1,085 °C Brazing iron and steel in a clay packet

Tin is smelted from cassiterite (see Tin and Pewter), lead from galena (see Lead), zinc and brass in Zinc and Brass, and silver in Gold and Silver. A tin-lead solder has a "pasty" range between the two temperatures where it is part solid, part liquid; the 63 : 37 mix has none, so it freezes instantly — best for electrical joints, which must not be disturbed while setting.

Fluxes

Flux For Notes
Rosin Copper, brass, tinned surfaces, all electrical work Gentle, not corrosive; can be left on
Tallow Lead, pewter Animal fat; plumbers wipe joints with it
Zinc chloride ("killed spirits") Iron, steel, tinplate, brass, zinc Strong and corrosive: wash it off afterward. Never on electrical work
Sal ammoniac (ammonium chloride) Cleaning and tinning the soldering iron A block you rub the hot iron on
Borax All brazing and silver soldering Must be dried by heating first

Tools

Item Notes
Soldering irons Two copper bits: about 150 g for wire and small work, 300–500 g for sheet seams (below)
Small brazier or forge A clean charcoal fire with no smoke — see Blacksmithing
Files, scrapers, sandstone For cleaning surfaces bright
Iron ladle For melting and alloying solder
Iron binding wire, clamps To hold parts in place
Small brush or feather To apply liquid flux
Clay, fine charcoal powder For brazing packets

Where to find it

  • Rosin: collect pine resin from cuts in pine bark. Heat it gently in a pot (outdoors — it is flammable) until the sharp-smelling turpentine has boiled off and a drop on a cold stone sets hard and glassy, amber to brown. Better, distil the turpentine off with water (see Distillation) and keep it. Powder the rosin, or dissolve it in alcohol for a liquid flux.
  • Tallow: render animal fat (see Lamps and Candles).
  • Zinc chloride: dissolve scraps of zinc in Hydrochloric Acid — outdoors, in a glass or glazed pottery jar, a little zinc at a time — until it stops fizzing and a little zinc is left undissolved. Let it settle and pour off the clear liquid. The fizzing gas is hydrogen, which burns explosively: no flames nearby. Adding a little sal ammoniac makes it work better.
  • Sal ammoniac: white crusts around volcanic steam vents and above burning coal seams. It was also made in Egypt for centuries from the soot of burnt camel dung, and can be made from ammonia and hydrochloric acid (see Ammonia). It vanishes into white smoke when heated, without melting.
  • Borax: white crusts and beds on the floors of dry salt lakes in deserts — Tibet, the Andes, western North America, Turkey. Heated on a hot iron, a crystal puffs up into white foam and then melts into a clear glass bead. Before use, heat it in a clay dish until it stops foaming, let it cool, and grind it fine: this is fused borax, which will not bubble on the work. Mix with water to a paste.

Making a soldering iron

Wooden handle Iron rod 25–35 cm Copper bit 150–500 g Tinned faces bright silver coat of solder Right heat · never glowing red · rosin smokes, no flame · solder melts at once Section across a lap seam lap 5–6 mm fillet solder fills the gap shows on the far side Running the seam solder fed in front 2–3 cm a second bright, smooth seam
Fig. 1 A soldering iron and its use. The copper bit stores heat; it is drawn slowly along the seam with solder fed in front of it, so the solder runs into the lap and through to the other side.

A soldering iron is a lump of copper on an iron rod. Copper holds a lot of heat and is wetted by solder, so it carries heat to the joint and lays solder along it.

  1. Cast or forge a block of copper (see Copper Smelting) about 2 × 2 × 6 cm for a 200 g bit, or larger for heavy work.
  2. Forge one end to a blunt four-sided pyramid point, or a hatchet shape — a wedge set crosswise — for long seams.
  3. Punch or drill a hole in the other end and fit an iron rod 6–8 mm thick and 25–35 cm long, riveted or screwed in tight. Fit a wooden handle on the other end.
  4. Tin it. Heat it in the fire, file the faces of the point bright, and immediately rub them on a block of sal ammoniac or in rosin together with a little solder. The faces should become a bright, mirror-silver coat of solder. A properly tinned bit picks up and carries solder; a dirty one will not.

Judging the heat. Heat the bit in a clean charcoal fire, never in smoky flame. It must never glow red — that burns off the tinning. It is right when:

  • held 10–15 cm from your cheek, you feel strong heat;
  • touched to rosin, it makes thick smoke but the rosin does not burst into flame;
  • solder touched to it melts instantly and runs over the tinned face.

If a green flame plays round the copper in the fire, it is far too hot. Work with two irons, one heating while you use the other.

Method 1: Soft soldering a sheet seam

  1. Prepare the joint. Overlap the sheets 5–6 mm, or better, fold them into a lock seam (see Sheet Metal and Rolling) so the joint holds by itself.
  2. Clean. Scrape or file both surfaces bright along the whole joint, inside the lap too. Do it just before soldering; fresh metal tarnishes within hours.
  3. Flux. Brush on zinc chloride (iron, tinplate, brass) or sprinkle rosin (copper, tinned surfaces).
  4. Tack. Hold the pieces together and touch the hot, loaded iron to the seam every 5 cm, so small spots of solder hold everything in line.
  5. Run the seam. Lay the flat face of the iron on the seam, wait two or three seconds for the metal under it to heat, then draw it slowly along — about 2–3 cm per second — feeding solder in front of the bit. Watch the solder flash into the lap. On thin sheet it should show as a bright line on the far side too.
  6. Do not move the work until the solder has set: shiny to slightly dull, in a few seconds.
  7. Wash off zinc chloride with plenty of water, then dry. Rosin can stay.

Method 2: Wire joints

  1. Bare and clean 4–5 cm of each wire end until bright (see Copper Wire).
  2. Twist. Cross the wires at their middles and wrap each end tightly around the other wire, 5–6 turns each way. This telegraph splice is strong on its own; the solder only makes the contact permanent and keeps air out.
  3. Flux with rosin only.
  4. Heat from below, solder from above. Hold the hot iron under the joint and touch the solder to the top of the joint, not to the iron. When the wire is hot enough, the solder melts and soaks right through the twist.
  5. Hold still until it sets. A good joint is bright and smooth and you can still see the shape of the wires under the solder.
  6. Insulate it (see Copper Wire).

Method 3: Pipes

  • Copper pipe (sweated socket joint). Open the end of one pipe on a tapered mandrel so the other slides in with a close fit, overlapping by one to two pipe diameters. Clean both, flux, push together, and heat the whole joint evenly in a clean charcoal fire or with a blowpipe flame. Touch solder to the edge of the joint: when hot enough, it is sucked in all the way round. Do not overheat — if the flux turns black, clean and start again.
  • Lead pipe (wiped joint). Plumbers taper one pipe end and flare the other so they fit together, clean them, and smear tallow round them. Molten plumber's solder is poured over the joint and, while it is pasty, shaped into a smooth bulb with a thick greased pad of cloth or leather. This takes real skill; the long pasty range of 1 : 2 tin-lead solder is what makes it possible. See Lead for the hazards.
  • Drinking water and food must use pure tin or tin-copper solder, never lead.

Method 4: Brazing

Spelter in the open fire section through a pipe socket Copper in a clay packet section through a lapped joint Close gap 0.05–0.15 mm Spelter grains in borax paste Heat the whole joint to bright red-orange; the spelter melts and is sucked into the gap. fire Copper strip along the joint Clay + charcoal 1–2 cm thick iron Heat to bright yellow (1,100–1,150 °C) for a few minutes; cool; break off the clay.
Fig. 2 Brazing. Left: a close-fitting joint wired together, painted with borax and set with spelter, heated until the spelter flashes into the gap. Right: brazing iron with copper inside a sealed clay packet.

With spelter or silver solder (in the open fire)

  1. Fit the parts with a close gap — 0.05–0.15 mm. Clean them bright and bind them with iron wire.
  2. Flux the joint with fused borax paste.
  3. Place the brazing metal — grains, filings or a thin strip of spelter, or small snippets of silver solder — along the joint, with a little more borax.
  4. Heat the whole joint in a clean charcoal fire, out of the direct blast. First the borax bubbles and dries, then melts into a clear glassy film (dull red, about 750 °C). Keep heating. At a bright red to orange heat for spelter (or a dull to cherry red for silver solder), the metal suddenly melts and flashes into the joint as a bright line. Stop as soon as it has run all the way along.
  5. Cool slowly. Chip and scrub off the glassy borax, or soak the part in hot water overnight.

Warning Zinc fumes. Overheated brass gives off white smoke of zinc oxide. Breathing it causes metal fume fever — shivering, aching and fever some hours later, like a bad flu. Braze in the open, upwind, and do not keep heating once the spelter has run.

With copper (the clay packet)

For joints in iron or steel where you cannot see inside — pipe sockets, tool joints, the seams of a sheet-iron bell or pot — wrap the work so air cannot reach it:

  1. Fit and bind the joint closely. Lay thin copper wire, strip or filings along it.
  2. Coat with borax paste if you have it.
  3. Wrap the whole joint in clay mixed with fine charcoal powder, 1–2 cm thick, and let it dry.
  4. Heat it in the forge to a bright yellow (1,100–1,150 °C) and hold it there for a few minutes after the packet glows evenly, turning it so the copper runs all round.
  5. Let it cool, then break off the clay. The copper will have flowed into every seam.

Even without borax, the charcoal inside a well-sealed packet keeps the surfaces from oxidising, and the joint usually takes.

Making solder

  1. Melt the tin first in an iron ladle. At about 250–300 °C a dry pine shaving pushed into it turns brown.
  2. Add the lead, weighed out in the right proportion. Stir with a green stick, which bubbles and stirs the melt.
  3. Skim the grey dross (oxide) off the top.
  4. Pour into grooves about 6 mm wide cut in a dry hardwood board, a stone, or a block of charcoal, to make sticks. For fine work, hammer or roll sticks into thin strip and cut it into narrow ribbons.

How to tell it worked

  • The look. A good soft-soldered joint is smooth and bright, with a concave fillet (a curved edge) where the solder meets the metal, as if it had been poured in. Solder that sits in round balls with sharp edges did not wet the metal.
  • Through the seam. On a lap joint, a thin line of solder shows on the far side.
  • Watertight. Fill a soldered vessel with water and stand it on dry paper overnight. No damp spots.
  • Wire joints. Pull hard: the wire should break before the joint. Electrically, a good joint makes no difference to how brightly a bulb glows across it.
  • Brazed joints. Clamp and bend a test piece: the metal should bend before the joint opens. Brazed metal is the colour of brass or copper along the whole seam.

Note Troubleshooting. Solder balls up and rolls off → dirty metal, no flux, or work not hot enough. Clean bright, flux again, and heat the work, not the solder. Joint dull, grainy and lumpy (a "cold joint") → the work moved while the solder set, or it was too cool. Reheat with fresh flux and hold still. Iron will not pick up solder → the tinning is burnt off: it got too hot. File it bright and re-tin it. Solder runs through and leaves a gap → gap too wide. Close it up, or lay more solder on. Spelter will not flow → not hot enough, or dirty. Heat further and add borax. Brazed joint full of pinholes → borax not fused before use, or the joint not cleaned. Soldered joint turns green or eats away → zinc chloride was not washed off.

Dangers

Danger Lead poisoning. Lead from solder enters the body mainly on your hands and food, not as fumes. Never eat, drink or smoke while soldering; wash your hands and face before eating; keep children away from the workbench and the scraps. Never use lead-bearing solder on anything that will hold food or drinking water. Lead poisoning is slow, silent and permanent — see Lead.

Danger Zinc chloride and acid. Hydrochloric acid and killed spirits burn skin and blind eyes. Make the flux outdoors, add the zinc a little at a time, and keep all flames away: the hydrogen given off explodes. Store it in a stoppered glass or glazed jar, clearly marked. If it splashes in the eyes, wash with clean water for 15 minutes.

  • Molten metal and water. A drop of water in a ladle of molten solder makes it spit violently. Keep moulds and tools bone dry; warm the moulds before pouring.
  • Burns. A soldering iron at working heat looks cold. Rest it on an iron stand, never on the bench.
  • Fumes. Rosin smoke irritates the lungs and can bring on asthma. Work where the air moves, and keep your face out of the smoke.
  • Zinc fumes from brass — see the warning above.

What this unlocks

Soldering makes possible tin cans (see Tins, Cans, Drums and Tanks), water Pipes, Plumbing and Aqueducts, lamps and kitchenware, fine Jewellery, Beads and Medals, and every electrical joint in Copper Wire, the The Telegraph, the The Telephone, Radio and circuit boards. Brazing gives strong joints for the The Bicycle, The Steam Engine fittings and tools. The next step in joining metals is true fusion Welding with gas and electric arc.

How it was first done

Goldsmiths at Ur in Mesopotamia were hard-soldering gold jewellery by about 2,500 BC, and Egyptian craftsmen soldered gold and silver and brazed copper. Etruscan and Greek goldsmiths joined grains of gold finer than sand to their work by heating them with a copper salt and glue, which forms a tiny solder joint in place. The Romans used tin-lead soft solder on a large scale for their lead water pipes; the Roman writer Pliny the Elder describes a solder of two parts lead to one of tin. Medieval European smiths brazed iron with copper and brass — the word braze is related to brass. Tinplate cans, sealed with soft solder, were patented in 1810, and soldered joints carried the electrical age from the telegraph of the 1840s to today's circuit boards.

Source: content/entries/metals/soldering-and-brazing.md