◆ Rebuild

Part 8 · Chemistry

Gelatin

The clean, edible heart of hide glue. Gently cooked out of fresh pig skin, calf hide or acid-softened bone, cleared through a jelly bag and charcoal, and dried as glassy sheets or ground to powder, gelatin sets desserts and aspics, makes medicine capsules and photographic plates, and was the first solid jelly for growing bacteria. This chapter covers the food and medical grades, and how to test them.

Difficulty
●●●●●
Time
An evening for calf's foot jelly; four to six days from fresh skins to dry gelatin sheets
Steps from zero
18 prerequisites →

You need first

Glues and AdhesivesButchery and Meat

This unlocks

Agar and Culture PlatesMaking Photographic Papers and Plates
The full path from nothing — 18 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Tar, Pitch and Glue
  12. Bellows
  13. Glues and Adhesives
  14. Iron (the Bloomery)
  15. Blacksmithing
  16. Steel
  17. Axes, Chisels, Knives and Planes
  18. Butchery and Meat
  19. Gelatin

Do them roughly in this order. See it on the tech tree →

Why it matters

Hide glue and gelatin are the same substance. Glue is the dark, smelly, strong-tasting form, good enough for joinery (Glues and Adhesives). Gelatin is the clean form: made from fresh, wholesome food scraps, extracted gently, cleared until it is nearly colourless, and dried hygienically. That difference opens a long list of uses:

  • Food. Clear fruit and wine jellies, meat aspics that seal and preserve cooked meat, soft sweets, marshmallow, and stiffened creams. Gelatin also turns tough, cheap parts of an animal — feet, skin, ears, bones — into nourishing food.
  • Medicine. The two-piece capsules that hide the taste of bitter drugs (Pharmacy: Tablets, Capsules, Ointments and Inhalers), soft capsules for oils, and the base of some pessaries and sutures.
  • Photography. The silver-bromide dry plate, film and photographic paper are all a thin layer of gelatin holding the light-sensitive crystals (Photography, Silver Nitrate and Silver Salts).
  • Microbiology. Gelatin set with meat broth was the first solid jelly on which bacteria could be grown as separate colonies (Culturing Microbes).
  • Craft and industry. Sizing fine paper (Paper), fining cloudy beer and wine (Beer, Wine and Cider), and light-hardened gelatin resists for printing plates and circuit boards (Integrated Circuits).

How it works

Skin, tendon and bone are held together by collagen: long protein chains twisted in threes like rope, bundled into tough fibres. Collagen does not dissolve in cold water. Warm it gently in water and the three-strand ropes come apart into single chains. That is gelatin.

Dissolved warm, the single chains float freely: a runny liquid. As it cools below about 25 °C, stretches of the chains try to twist back into three-strand ropes with their neighbours. They catch hold of each other at thousands of points and form a fine net that traps all the water: a jelly. Warm it again above about 30–35 °C and the net unknots. This is why a good jelly melts on the tongue, just below body heat.

Three things follow:

  1. Long chains make strong jelly. Every step that breaks the chains — boiling, long heating, strong acid or alkali, bacteria — weakens the jelly. The first, gentlest extraction gives the best gelatin; later, hotter runs give glue.
  2. The raw material must first be loosened. Fresh skin is held together by cross-links that resist heat. A pre-treatment loosens them:
    • Acid for a few hours to a day, used for young pig skin, gives type A gelatin: clear, quick to make, the usual food gelatin.
    • Lime for weeks or months, used for tough cattle hide and bone ossein, gives type B: slower to make, slightly stronger and more neutral, the usual photographic and much pharmaceutical gelatin.
  3. Enzymes destroy it. Raw pineapple, papaya, kiwi fruit, fig and fresh ginger contain enzymes that cut protein chains. A jelly made with their raw juice never sets. Cooked or canned, they are harmless.

The strength of a jelly is measured in bloom (after its inventor, Oscar Bloom): the grams of weight needed to press a small standard plunger 4 mm into a standard jelly. Good food gelatin is 150–250 bloom; glue is under 100.

What you need

Item Amount Notes
Fresh pig skin or calf or cattle hide trimmings 5 kg Clean, unsalted, never tanned or limed by a tannery. From animals killed for food (Butchery and Meat)
Or calves' or pigs' feet 4 feet For kitchen jelly (Method 1)
Or bone ossein 2–3 kg Bone softened in dilute acid (Hydrochloric Acid)
Hydrochloric or sulfuric acid Diluted to about 2 % for pig skin (Hydrochloric Acid, Sulfuric Acid)
Slaked lime 1 kg per 20 litres of water For hide and ossein (Lime)
Eggs 2–3 whites per 2 litres For clarifying
Bone char or activated charcoal 20–40 g per litre For decolourising (Activated Charcoal)
Vessels Glazed stoneware, enamelled iron (Enamel on Metal) or tinned copper (Pots, Pans and Kettles); never bare iron (turns gelatin grey) or zinc
Thermometer Strongly advised (The Thermometer)
Jelly bag See below
Glass sheets or tinned trays, drying nets Fine cotton or linen netting on frames

Where to find it

Everything comes from the slaughter of healthy animals (Butchery and Meat). Pig skin gives the clearest, quickest gelatin — the fat must be scraped off first. Calves' feet and pigs' trotters give the richest kitchen jelly. Cattle hide trimmings (the edges cut off before tanning, Hides and Leather) and bones give the most by weight. Fish skins give a weaker jelly that melts at room temperature, useful for some sweets and fining.

Method 1: Calf's foot jelly (the kitchen way)

This is how households made gelatin dessert and invalid food for centuries, with no chemicals at all.

  1. Prepare. Scald 4 calves' feet or 6 pigs' trotters in boiling water, scrape off hair, and split them lengthways between the toes with a cleaver.
  2. Simmer them in 4 litres of water very gently — the surface just trembling — for 6–8 hours, until the water has reduced to about 2 litres and the meat falls from the bones.
  3. Strain through a coarse cloth into a clean bowl and leave it overnight somewhere cold. It sets into a firm, cloudy jelly with fat on top.
  4. Remove the fat completely: scrape it off, then wipe the surface with a cloth wrung out in hot water. Scrape off any sediment at the bottom.
  5. Clarify (below), sweeten and flavour it, and set it in a mould.

Two litres of this stock hold roughly 40–60 g of gelatin — enough for a firm moulded jelly.

Clarifying with egg white

Cloudy stock or gelatin liquor is full of tiny particles that no cloth will hold. Egg white catches them.

  1. Melt the jelly over low heat. For each 2 litres, whisk 2–3 egg whites with their crushed shells and a cupful of the cool liquid, and stir it in while the liquid is still lukewarm.
  2. Heat slowly, without stirring, to a gentle simmer. As the egg white cooks it rises as a grey crust, carrying the particles with it.
  3. Simmer 5 minutes, then turn off the heat and let it rest 10 minutes.
  4. Ladle it gently through the jelly bag without breaking the crust more than you must. Pour the first, cloudy cupful back through. What drips out is clear and bright.

The jelly bag

A jelly bag is a cone of tightly woven, napped cloth — flannel, felt or thick twilled cotton — that filters slowly by its own weight. Cut a quarter-circle of flannel with a radius of 40 cm and sew the two straight edges together to make a cone about 40 cm deep and 25 cm across the mouth, with the fluffy side inside. Sew a ring of cord or a wire or willow hoop into the mouth with four loops, and hang it from a stool turned upside down, or a frame, over a bowl. Scald it in boiling water before each use, and wring it out hot: a hot bag lets jelly through before it sets. A good bag gives a first cloudy cupful and then a steady clear drip; a bag that runs fast and cloudy is too thin — use two layers.

1. Clean skin strips2 % acid, 12–24 hours;then wash to pH 4–5(or lime for weeks: hide, bone) 2. Extract in runsnever boiling; keep separate 1st 55–60 °Cbest gelatin2nd 65–70 °Cfood grade3rd 75–80 °C+stock, glue 3. Clarifyegg white, bone char,scaldedflanneljelly bagclearliquor concentrate below 60 °C; heat once to 80–85 °C 4. Cast 3–4 mm thinon glass; set cold, cut intoleaves about 7 × 22 cmglass sheet 5. Dry on cotton netsbreeze; below 20 °C at first;2–3 days→ gelatin sheets 6. Or press intonoodles3–5 mm holes; dry,grind, sieve→ gelatin powder
Fig. 1 Making clear gelatin. Pre-treated skins are extracted in several runs at rising temperatures; the best first run is cleared with egg white, bone char and a jelly bag, cast thin and dried on nets as sheets, or pressed into noodles and ground to powder.

Method 2: Sheet gelatin from pig skin

This gives the clean, pale, food and medical grade.

  1. Clean. Scrape all fat from 5 kg of fresh pig skin, and shave or scald off hair. Cut it into strips 2–3 cm wide.
  2. Acid soak. Soak the strips in dilute acid of about 2 % — about 70 ml of strong (30 %) Hydrochloric Acid in 1 litre of water — using about 3 litres per kg of skin, for 12–24 hours in a cool place, stirring now and then. The skin swells and turns translucent. (Type A gelatin.)
  3. Wash in many changes of clean water over half a day, until the water tests only faintly acid: pH 4–5 on a test paper (cabbage indicator just turning from red to purple, pH, Indicators and Buffers).
  4. First run. Just cover the skins with clean, soft, boiled-and-cooled water and heat to 55–60 °C — uncomfortably hot to a finger but far from steaming. Hold it there 4–6 hours, stirring gently. Draw off the liquor. This is the best gelatin.
  5. Later runs. Add fresh water, extract at 65–70 °C, then 75–80 °C, then near boiling. Keep each run separate. The later runs are darker and weaker: use them for cooking stock, sizing and glue.
  6. Clarify the first run with egg white, as in Method 1, or let it stand hot (above 60 °C) for 2 hours so solids settle, and pour off the clear part.
  7. Decolourise if it is yellow: stir in 20–40 g of bone char or activated charcoal per litre, hold at 60 °C for 30 minutes, and filter through paper or a double jelly bag (Activated Charcoal).
  8. Concentrate. Heat the clear liquor in a shallow, wide pan at no more than 60 °C, uncovered, with a breeze over it, until a drop on a cold plate sets firm in a minute (about 15–20 % gelatin).
  9. Pasteurise. Bring it once to 80–85 °C for 5 minutes to kill bacteria, then cool it quickly. This costs a little strength but makes it safe to store.
  10. Cast. Pour it 3–4 mm deep onto level glass sheets or tinned trays wiped with a trace of oil, or onto wet glass. Let it set in a cold room for 2–3 hours.
  11. Cut the set film into leaves — the usual size is about 7 × 22 cm — with a wetted knife.
  12. Dry the leaves on taut cotton nets in a clean, airy, shaded room, away from flies and dust. Start them cool (below 20 °C): warm air melts a wet leaf onto the net. After a day, when they feel leathery, they can take 25–30 °C. They are dry in 2–3 days: glassy, brittle, snapping cleanly. The faint diamond pattern of the net stays in them.

Yield: roughly 400–600 g of dry gelatin from 5 kg of fresh pig skin, about half of it first-run quality.

Gelatin sheets

A good gelatin sheet is thin, even, transparent and nearly colourless, and snaps cleanly. A standard leaf weighs 2–3 g; weigh ten of your own and note the average so recipes come out right. Bend-test: a dry leaf that bends without snapping still holds water and will go mouldy — dry it longer. Yellow or brown leaves came from a later run or were dried too warm. Leaves that smell of glue when wetted came from stale skin, or were too slow to dry.

Gelatin powder

Gelatin powder dissolves faster and measures by the spoon.

  1. Instead of casting thin, let the concentrated liquor set 2–3 cm deep in a tray.
  2. Press the cold, firm jelly through a perforated tinned plate or coarse sieve with 3–5 mm holes into short noodles, letting them fall onto a drying net.
  3. Dry them as for leaves, then a final day at 30–35 °C.
  4. Grind in a clean hand mill or mortar and sieve. Store airtight.

A level tablespoon of powder is about 9 g, and a level teaspoon about 3 g. Good powder is pale, free-running, odourless, and wets and swells without lumps when sprinkled on cold water.

Method 3: From bone ossein (type B)

Make ossein from clean bones by dilute acid (Hydrochloric Acid). Then lime it: soak in lime water (1 kg slaked lime per 20 litres) for 4–8 weeks, changing the lime water every week, until it is plump and white. Wash out the lime for 1–2 days, finishing with a bath of very dilute acid to pH 5–6. Then extract, clarify and dry as in Method 2. Bone gelatin is slower to make but very consistent, and was long the gelatin of photography and capsules.

Grades

Grade Made from Requirements
Food First and second runs, fresh skin or bone Bloom 150–250; pale; no smell or taste; clean drying
Pharmaceutical First runs only Bloom 150–280; very clear and pale; pasteurised; no mould; dissolves completely; tested on a sample batch of capsules (Pharmacy: Tablets, Capsules, Ointments and Inhalers)
Photographic Limed bone or hide Tested by making an emulsion from each batch; traces of impurities change film speed (Photography)
Technical Third and later runs Glue, sizing (Glues and Adhesives, Paper)

Testing: the bloom gauge

Cup pour in lead shot or sand Wooden bridge two guide holes keep the rod upright Pointer and mm scale stop when it has moved 4 mm Standard jelly 7.5 g gelatin + 105 ml water, jar 6 cm across, 17 hours at 10 °C Plunger rod flat, square end 12.7 mm across Result rod + cup + shot, in grams = bloom food gelatin: 150–250 4 mmtip pressed in
Fig. 2 The bloom gauge. A flat-ended rod rests on a standard jelly; shot is poured into a cup on top until the rod sinks 4 mm. The weight of rod, cup and shot in grams is the bloom strength.

To make a reliable product you must measure its strength. Build a bloom gauge:

  1. The jelly. Dissolve 7.5 g of gelatin in 105 ml of water (6.67 %) at 60 °C. Pour it into a straight-sided glass jar about 6 cm across, to about 3 cm deep. Cover and hold at 10 °C (a cold cellar or spring house, Ice and Refrigeration) for 16–18 hours.
  2. The plunger. A smooth, straight rod of hardwood or brass, with its end filed flat and square: 12.7 mm across (half an inch). It slides freely and upright through two holes in a wooden bridge that stands over the jar. Fix a light cup or tin on top of the rod, and a pointer on the rod that moves against a scale marked in millimetres on the bridge post.
  3. The test. Lower the plunger until it just touches the jelly surface; note the pointer. Pour lead shot or fine sand steadily into the cup until the pointer has moved 4 mm. Weigh rod, cup and shot together on a balance (Balances, Steelyards and Weighing Machines). That weight in grams is the bloom.
  4. Repeat with three jars and average. Results within 10 % of each other are good.

Without a gauge, compare against a reference batch you have kept. Make both into 2 % jellies in identical cups, chill them together, and press each with the same fingertip: you will feel a 20 % difference.

Other tests:

  • Clarity: a 5 % solution in a clear glass 5 cm deep lets you read print through it.
  • Smell: warm a spoonful of solution and sniff: good gelatin smells of nothing; bad smells of glue or meat.
  • Melting: a cube of firm jelly held on the palm melts in a minute or two.
  • Ash: burn 5 g in a crucible: less than 0.1 g of ash should remain. Much more means lime or acid was not washed out.

Using gelatin

To use sheets: soak in plenty of cold water for 5–10 minutes until floppy, squeeze, and stir into warm liquid (50–60 °C, never boiling). To use powder: sprinkle onto five times its weight of cold water, wait 5 minutes ("blooming"), then melt into warm liquid.

Use Gelatin in the finished liquid
Soft dessert jelly, served in the glass 1.5–2 % (8–10 g per 500 ml)
Firm jelly to turn out of a mould 2.5–3 %
Meat aspic, glaze for cold meat 3–5 %
Marshmallow 2.5–3 % of the whole batch
Gummy sweets 7–10 %
Nutrient gelatin for bacteria 12–15 % in broth; grow at or below 22 °C
Hard capsules 35–40 % solution for dipping (Pharmacy: Tablets, Capsules, Ointments and Inhalers)
Photographic emulsion about 2–8 % (Photography)
Fining beer or wine about 0.01–0.02 % (Beer, Wine and Cider)

Very sour liquids (lemon, vinegar, sour fruit) and wine need about 20 % more gelatin.

The gelatin dessert

  1. Warm 500 ml of fruit juice or wine with 50–100 g of sugar (Sugar) to about 60 °C. Squeeze in half a lemon (Citric and Tartaric Acid) for brightness.
  2. Stir in 12–15 g of gelatin (soaked sheets or bloomed powder) until fully dissolved. Strain through a cloth.
  3. Rinse the jelly mould with cold water, pour in, and set somewhere below 10 °C for 4–6 hours or overnight.
  4. To turn out, dip the mould in hot water for 5 seconds, put a plate over it, and invert.

A jelly mould is any smooth, slightly flaring vessel with no undercuts: glazed earthenware (Pottery), tinned copper or pressed tin (Sheet Metal and Rolling), or glass, 0.5–1 litre. Fluted moulds look grand but need firmer jelly (3 %). A good mould releases cleanly with sharp ribs; a rough, crazed or undercut one tears the jelly.

How to tell it worked

  • Dry gelatin is glassy, pale amber to colourless, brittle, and odourless.
  • A 2 % solution sets to a firm jelly in 4 hours below 10 °C, and melts on the tongue.
  • The bloom gauge reads 150 or more for food and medical use.

Note Troubleshooting. Liquor will not set even when concentrated → it was boiled, held hot too long, went sour, or the skins were over-acid. Extract cooler, faster and cleaner. Jelly is cloudy → fat or fine particles: degrease, settle hot, clarify with egg white, and filter through a scalded bag. Leaves melted onto the nets → drying air too warm at the start. Begin below 20 °C. Leaves went mouldy or slimy → drying too slow in damp, still air. Dry in a breeze, in cool dry weather, or cast thinner. Dessert did not set → raw pineapple, papaya, kiwi, fig or ginger; or too little gelatin for an acid juice. Tastes of glue → stale or tannery-touched raw material, or a later run. Use first runs from fresh skins.

Dangers

Danger Disease from the raw material. Use only skins and bones from healthy animals killed for food and inspected (Butchery and Meat, Animal Health). Animals that died of disease can carry anthrax, whose spores survive boiling. Where mad cow disease (BSE) has occurred, never use the skull, brain, spinal cord or spine of cattle, or bones of older cattle; pig skin is the safest source.

Warning Warm gelatin is a perfect food for germs. Anywhere between about 5 °C and 60 °C, and fastest between 20 °C and 50 °C, gelatin liquor and jelly spoil in hours and can grow food-poisoning bacteria. Keep liquor hot (above 60 °C) or cold, as cold as you can, ideally below 5 °C; never leave it lukewarm for long. Eat desserts and aspics within 3 days, kept cold. Meat aspic is meat, and needs the same care (Preserving Food). Dry gelatin keeps for years.

What this unlocks

How it was first done

Cooks have made jellies from calves' feet, pig skin and fish swim bladders since at least the Middle Ages; aspic and calf's foot jelly were feast dishes and invalid food in Europe. In 1682 the French physicist Denis Papin showed his pressure "digester", which cooked bones into jelly. In the early 1800s French chemists, among them Jean d'Arcet, extracted gelatin from bones with acid to feed hospitals and the poor. Peter Cooper in the United States patented a powdered gelatin dessert in 1845, and Jell-O followed in 1897. Gelatin capsules were patented in France in 1834 and the two-piece hard capsule in 1846. Richard Maddox described the gelatin silver-bromide dry plate in 1871, and Robert Koch grew bacteria on gelatin plates in 1881, before his laboratory switched to Agar and Culture Plates.

Source: content/entries/chemistry/gelatin.md