A beginner's geology for people who need stone, not degrees. How rocks form, how to read a landscape for the ones you want, and how to identify minerals with a fingernail, a copper bead, a knife, a piece of pottery and a drop of vinegar.

Difficulty
●●●●●
Time
An afternoon to make a test kit; a lifetime to get good at it, but useful from the first day
Steps from zero
0 prerequisites →

You need first

Nothing — start here.

This unlocks

Zircon and Zirconium

Why it matters

Every material in this book that does not grow comes out of the ground. You need limestone for Lime, clay for Pottery and Bricks, sand of the right kind for Glass, flint for Stone Tools, sandstone for whetstones, gypsum for Gypsum and Plaster of Paris, heavy coloured stones for metal (Finding and Identifying Ores), and good solid rock to build with (Quarrying and Cutting Stone). A person who cannot tell one rock from another walks past all of these every day.

The good news is that you do not need to know hundreds of minerals. About twenty common rocks and minerals make up almost everything you will meet, and a handful of simple tests — scratch, streak, shine, weight, fizz — tell them apart. This chapter teaches those tests and how to read the landscape so you know where to look before you even pick up a stone.

How it works

Minerals and rocks

A mineral is a natural substance with a fixed chemical make-up and, usually, a regular crystal structure: quartz, calcite, gypsum, mica, feldspar. A rock is a mixture of one or more minerals stuck together. Granite, for example, is a rock made of quartz, feldspar and mica grains. Limestone is a rock made almost entirely of the mineral calcite.

The three families of rock

All rock forms in one of three ways, and knowing which family a rock belongs to tells you what else to expect nearby.

Igneous: lavacooled fast at the surface —basalt, obsidian, pumice Riverpebbles of everythingupstream Sedimentarylayers: sandstone, shale,limestone (with fossils) Baked zonerock next to the hot granite Metamorphiccooked and squeezed deep:slate, schist, quartzite Igneous: granitecooled slowly underground —crystals big enough to see
Fig. 1 The three families of rock in one landscape. Igneous rock cools from melt; sedimentary rock settles in layers from water; metamorphic rock is either of these cooked and squeezed deep underground. Each sends its own pebbles down the river.
  1. Igneous rock (from the Latin for fire) cooled from molten rock. If it cooled slowly deep underground, its crystals had time to grow big enough to see: granite (speckled white, pink, grey and black) and its relatives. If it cooled fast at the surface as lava, the grains are too fine to see: basalt (dark, heavy). Lava that cooled instantly becomes natural glass, obsidian; lava frothed full of gas becomes pumice, which floats. Igneous rocks have no layers and no fossils.
  2. Sedimentary rock formed from loose material — sand, mud, shells, salt — that settled in water or on land and was slowly pressed and cemented into stone. Sandstone (cemented sand), shale (hardened mud, splits into thin flakes), limestone and chalk (shells and lime mud), conglomerate (cemented pebbles), coal (buried plants), rock salt and gypsum (left by drying seas). They lie in layers (beds), often contain fossils, and are where you find most of the materials for building and chemistry.
  3. Metamorphic rock is any rock changed by heat and pressure deep underground without melting. Shale becomes slate (splits into flat sheets), then schist (glittering with mica). Limestone becomes marble (sugary crystals, still fizzes with acid). Sandstone becomes quartzite (extremely hard; breaks through the grains, not around them). Metamorphic rocks often have their minerals lined up in streaks or bands, and many ore veins are found in them.

Rocks are always being turned into one another: mountains wear down into sand, sand becomes sandstone, sandstone is buried and cooked into quartzite, and so on. You do not need the theory, but it explains why certain things are found together.

What makes minerals different

Every mineral has properties you can test with no instruments:

  • Hardness — what it scratches and what scratches it.
  • Streak — the colour of its powder.
  • Lustre — how its surface reflects light.
  • Cleavage — whether it splits along flat planes, and how many.
  • Heft — how heavy it feels for its size (density).
  • Reaction to acid — whether it fizzes.

Colour alone is unreliable. Quartz can be white, clear, pink, purple, smoky or black. Use the tests.

What you need

Item What for How to get it
Hammerstone Break rocks to see a fresh face A fist-sized tough river cobble (see Stone Tools)
Streak plate See the colour of a mineral's powder The unglazed base of a fired pot or a piece of broken tile (see Pottery)
Hardness set Scratch tests Fingernail; a bead or wire of copper; an iron nail or steel knife; a piece of glass or a glazed sherd; a quartz pebble (see table below)
Acid The fizz test Strong vinegar; better, vinegar boiled down to half its volume (see Fermentation); later, dilute Hydrochloric Acid
Lodestone Find magnetic minerals See Finding and Identifying Ores and Magnets
Hand lens See small grains Optional; any lens (see Lenses). A drop of water on a leaf also magnifies a little.
Bags and labels Carry samples and remember where they came from Leather pouches, cloth, Baskets and Containers; a charcoal mark on a pebble

Where to find it: reading a landscape

Geology starts with your eyes from a distance. Learn these clues and you will know roughly what lies underfoot before you dig.

You see… It probably means… Useful for
Cliffs and hillsides in flat or tilted stripes Sedimentary rock (sandstone, shale, limestone) Building stone, clay, lime, coal, salt
Pale grey or white cliffs; caves, sinkholes, streams that vanish underground; springs leaving white crusts Limestone (karst country) Lime, Mortar and Concrete, Portland Cement, flux for Iron (the Bloomery)
Smooth white rolling hills, white sea cliffs with black lumps Chalk with flint nodules Lime, flint for Stone Tools
Rounded domes, boulders and tors of speckled rock; sandy, acid, peaty soils; clear streams Granite Building stone, querns, tin and kaolin (white clay) in streams
Black cliffs in six-sided columns; dark, heavy cobbles; fertile dark soils Basalt and old lava Ground axes, Abrasives and Grinding Stones, querns, pozzolan ash nearby
Cone-shaped hills, hot springs, yellow crusts, sulphur smell Volcanic country Sulfur, volcanic ash for concrete, pumice, obsidian, hot water (Geothermal, Tidal and Wave Power)
Hillsides of rock that splits into thin flat grey slabs Slate Roofing, flooring, writing slates
Rock with glittering flakes, wavy bands, white quartz veins Metamorphic rock (schist, gneiss) Ore veins, mica, garnet
Red or orange soil and rock, rusty seeps Iron oxide Finding and Identifying Ores, red pigment (Pigments, Paints and Varnish)
Grey, sticky soil in valley bottoms; ponds that never drain Clay Finding and Preparing Clay, Bricks
White crusts in dry hollows; salty or bitter springs Evaporites — salt, gypsum, soda Salt, Gypsum and Plaster of Paris, Soda Ash and Baking Soda
A line of springs and wet ground along a hillside Permeable rock (sandstone, limestone) sitting on watertight rock (shale, clay) Finding and Purifying Water, Wells and Cisterns

Let the rivers do the walking. A stream bed is a free sample of everything upstream. Note what pebbles you find. Walk upstream; when a kind of pebble stops appearing, its source is just above that point, often up a side valley. This is how prospectors have always found ore and good stone.

Follow the layers. Sedimentary beds stretch for kilometres. If you find a good limestone or a clay bed in one valley, look for the same layer at the same height in the next one — or on the same slope, where the angle of tilt carries it.

Look at old work. Ruins, old quarries, mine dumps and road cuttings show fresh rock that would otherwise be hidden under soil.

The field tests

Always test a fresh, clean surface. The outside of most rocks is weathered, stained and softened. Break it with your hammerstone, wearing eye protection (see Dangers).

1. Hardness

Hardness is how easily a mineral is scratched. Geologists use the Mohs scale from 1 (softest) to 10 (hardest), named after the German mineralogist Friedrich Mohs, who set it up in 1812 using ten common minerals. Each one scratches all those below it.

Mohs hardness scale Each mineral scratches every one to its left. softerharder 12345678910 TalcGypsumCalciteFluoriteApatiteFeldsparQuartzTopazCorundumDiamond Fingernail2½ Copper3 Iron nail4½ Knife, glass5½ Steel file6½ Quartz pebble7 Softgypsum, talc,salt, mica, clay Mediumcalcite, limestone,marble, most ores Hardfeldspar, quartz, flint, chert —they scratch glass and steel
Fig. 2 The hardness scale with everyday test tools. Try to scratch the mineral with each tool from softest upward. The first tool that leaves a groove tells you the mineral is softer than that tool.
Mohs Reference mineral Field test Examples you will meet
1 Talc Greasy; your fingernail scratches it very easily Soapstone, graphite (1–2)
2 Gypsum Fingernail scratches it (fingernail ≈ 2.5) Gypsum, rock salt (2.5), clay minerals, mica (2.5–3)
3 Calcite Copper scratches it (copper ≈ 3); fingernail does not Limestone, marble; galena is just below, at 2.5
4 Fluorite Iron nail scratches it easily (nail ≈ 4.5) Fluorite, malachite, dolomite (3.5–4)
5 Apatite Knife scratches it with effort (steel knife ≈ 5.5) Hematite and magnetite (5.5–6.5)
6 Feldspar Scratches glass; a file scratches it (file ≈ 6.5) Feldspar in granite, pyrite (6–6.5)
7 Quartz Scratches glass and steel easily; nothing ordinary scratches it Quartz, flint, chert, quartzite
8–10 Topaz, corundum, diamond Scratch quartz Emery (corundum) — rare and valuable for Abrasives and Grinding Stones

How to do it. Press the point of the test tool firmly into a flat face of the mineral and drag it about 1 cm. Then rub the line with a wet finger. A real scratch is a groove you can feel with a fingernail. A soft tool rubbed on a hard mineral leaves a line of the tool's powder that wipes away. Test both ways: if A scratches B and B does not scratch A, A is harder.

With no metal at all, build a reference set of three stones: a piece of gypsum (2), a piece of calcite or limestone (3) and a quartz or flint pebble (7). That alone sorts most rocks into soft, medium and hard.

Rock versus mineral. Some rocks crumble — sandstone grains fall apart under a knife even though each quartz grain is hard. Scratch a single grain or crystal if you can, and remember that crumbling is not softness.

2. Streak

Rub the mineral firmly across your unglazed pottery. The colour of the powder is far more reliable than the colour of the lump:

  • Hematite is black, grey or red as a rock, but always gives a red-brown streak.
  • Magnetite gives black; bog iron and limonite give yellow-brown.
  • Pyrite ("fool's gold", brassy) gives greenish-black; real gold gives gold.
  • Most light-coloured, non-metallic minerals — quartz, calcite, gypsum, feldspar — give a white streak or none.

Minerals harder than about 7 are harder than the pottery and leave no streak; they scratch the plate instead.

3. Lustre

Turn the fresh face in the light. Describe it with one of these words:

Lustre Looks like Examples
Metallic Polished metal; opaque Galena, pyrite, magnetite, many ores
Glassy Broken glass Quartz, calcite, rock salt
Pearly Inside of a shell Gypsum and mica on their cleavage faces, talc
Silky A skein of silk Fibrous gypsum (satin spar), asbestos (see Dangers)
Waxy or greasy A candle or greased skin Flint, chert, soapstone, opal
Dull or earthy Dry soil Chalk, clay, red ochre, bog iron

4. Cleavage and fracture

Hit a mineral with your hammerstone and watch how it breaks.

  • Cleavage — it splits along flat, shiny planes, again and again in the same directions. Mica peels into one direction of thin, clear, bendable sheets. Gypsum also peels into thin sheets, but they snap instead of springing back. Rock salt and galena break into little cubes (three directions at right angles). Calcite breaks into slanting boxes called rhombs.
  • Fracture — it breaks with no flat planes. Quartz, flint and obsidian break in smooth curved shell shapes (conchoidal fracture) — this is what makes them good for sharp tools.

5. Heft

Hold the sample in one hand and an ordinary pebble of the same size in the other. Most common rocks are about 2.6–2.7 times as heavy as water. Gypsum is lighter (2.3), pumice so light it floats, coal light (1.3–1.5). Metal ores are much heavier (iron oxides about 5, galena 7.5). A stone that feels "wrong" — far too heavy — deserves a closer look (see Finding and Identifying Ores).

6. The acid test

Put a drop of strong vinegar on a fresh surface and watch closely, ideally with a lens.

  • Calcite (limestone, chalk, marble, shells) fizzes with tiny bubbles of carbon dioxide. Strongly with chalk, steadily with limestone.
  • Dolomite (a magnesium-rich limestone) fizzes only when scratched into powder first, or with warm acid.
  • Gypsum, quartz, flint, granite, basalt do not fizz at all.

Vinegar is weak; if you see nothing, scrape some powder into a spoonful of vinegar and warm it. Lemon or sour fruit juice works the same way.

7. Other quick tests

  • Magnetism — magnetite jumps to a lodestone (see Finding and Identifying Ores).
  • Taste — rock salt tastes salty, alum astringent, soda soapy. Only lick a mineral you are already fairly sure about; some, such as those with lead, arsenic or copper, are poisonous.
  • Feel — talc and graphite feel greasy; clay smells earthy when breathed on; shale smells of clay; some limestones smell of oil when struck.
  • Heat — a flake of gypsum heated on a hot stone turns white and opaque and gives off steam; calcite does not change at that heat.

Step by step: identifying an unknown stone

yesyesyesyes nononono Break it. Look at a fresh face. Shines like metal, very heavy,or a coloured streak? Fizzes with vinegar? Fingernail scratches it? Scratches glass? Probably an oreiron, copper, lead, tin —see Finding and Identifying Ores Calcite familychalk: soft, white, marks your fingerslimestone: layered, often with fossilsmarble: sparkling sugary crystals Softgypsum: no taste, no fizz, pearly or sugaryrock salt: tastes salty, breaks in cubestalc, soapstone: greasymica: peels into springy sheets Hardquartz: glassy, white or clear, no cleavageflint, chert: waxy, sharp curved breaksgranite: speckled interlocking crystalsbasalt: dark, heavy, grains too fine to seesandstone: gritty, grains rub off Mediumslate: splits into flat ringing sheetsdolomite: fizzes only when powderedshale, serpentine, weathered rock
Fig. 3 A simple key. Answer each question with a test from this chapter and follow the arrows. It will not name every rock on earth, but it sorts the common ones you need.
  1. Break it. Look at a fresh face. Note the colour, but don't decide yet.
  2. Grains or no grains? Can you see separate grains or crystals? Are they all the same, or a mixture (speckled)? Are they rounded (sand) or interlocking (crystals)?
  3. Layers? Does it split in layers, sheets or slabs?
  4. Scratch it with fingernail, copper and steel or quartz. Write down the hardness band.
  5. Streak it. Coloured streak usually means a metal ore.
  6. Acid. Fizz or no fizz?
  7. Heft. Normal, light or heavy?
  8. Compare with the table below, and keep a labelled sample of everything you identify. A reference collection is the fastest teacher.

Which rocks are useful for what

Rock or mineral How to know it Use it for
Flint, chert, obsidian Hardness 7 (obsidian 5.5), waxy or glassy, shell-shaped breaks Cutting tools, fire-striking (Stone Tools, Fire)
Basalt, dolerite Dark, heavy, fine-grained, tough; rings when struck Ground axes, hammerstones, querns, road stone
Granite Speckled interlocking crystals, hard, no layers Building, millstones, kerbs; source of tin and kaolin
Sandstone Gritty like sandpaper, layered, grains rub off Building stone, whetstones and grindstones (Abrasives and Grinding Stones), glass sand when crushed
Limestone and chalk Fizzes; scratched by steel (chalk by fingernail) Lime, Portland Cement, Glass, flux for smelting, building
Marble Sugary sparkling crystals; fizzes Lime, carving, fine building
Shale and mudstone Fine, soft, splits in thin flakes, smells of clay Weathers into clay; with limestone, raw material for cement
Slate Splits into flat hard sheets that ring Roofing, floors, writing slates
Quartz Hardness 7, glassy, no cleavage, white or clear Glass, flux, hard grit
Gypsum Fingernail scratches it; no fizz; pearly sheets or sugary white rock Gypsum and Plaster of Paris, fertiliser
Mica Peels into thin, clear, springy sheets Stove and lantern windows, electrical insulation (The Vacuum Tube, Wiring and Electrical Safety)
Soapstone (talc) Very soft, greasy, grey-green Carved pots, moulds for Metal Casting, griddles — it takes heat without cracking
Pumice and volcanic ash Very light, frothy or powdery Abrasive; pozzolan for Mortar and Concrete
Feldspar Pink or white blocky crystals in granite, hardness 6, two flat cleavages Stoneware and Porcelain, Glazes
Clay Sticky and plastic when wet Pottery, Bricks, Portland Cement
Coal Black, light, burns Fuel, coke (Coal and Coke)
Coloured, heavy, metallic stones Coloured streak, heavy Metals (Finding and Identifying Ores)

How to tell it worked

You are learning well when:

  • Your hardness results agree both ways (A scratches B, B does not scratch A).
  • Several tests point to the same answer. One test can mislead; three rarely do.
  • What you predict from the landscape turns out to be under the soil when you dig.
  • Stone you choose for a job behaves as expected: your "limestone" burns to quicklime that hisses in water (Lime); your "gypsum" turns to powder that sets (Gypsum and Plaster of Paris); your "flint" flakes sharp.

Note Troubleshooting. Everything seems to fizz → you are testing a weathered crust or soil with lime in it; break a fresh face. Nothing fizzes, even chalk → your vinegar is too weak; boil it down, or try warm acid on powder. "Scratches" that wipe off → the test tool left its own powder; rub with a wet finger and feel for a groove. Hardness changes from place to place → it is a rock (a mixture), not a single mineral; test individual grains. Brassy mineral, cannot decide gold or pyrite → gold is soft (a knife dents it, it bends), very heavy and gives a gold streak; pyrite is hard, brittle and gives a greenish-black streak.

Dangers

Danger Flying chips blind people. Rock and especially flint and quartz break into razor-sharp splinters that fly several metres. When breaking rock, look away at the moment of the blow, or shield your eyes with a leather or wooden visor, a hand, or a cloth. Keep others back.

  • Asbestos. A silky, fibrous mineral that pulls apart into soft threads (in green serpentine rock and some old buildings). Breathing its fibres causes deadly lung disease decades later. Do not break, crush or rub silky, fibrous minerals; leave them alone. Satin-spar gypsum also looks silky but is soft and dissolves slowly in water; if unsure, avoid it.
  • Dust. Grinding quartz, flint, sandstone or granite makes fine silica dust that scars the lungs (silicosis). Work wet, outdoors, upwind.
  • Poisonous minerals. Bright green, blue, red or yellow minerals, heavy grey metallic ones, and anything that smells of garlic when heated may contain copper, lead, mercury or arsenic. Do not lick, wash your hands after handling, and never heat unknown minerals indoors (see Finding and Identifying Ores).
  • Cliffs and cuttings. Rock faces drop stones without warning, especially after rain and frost. Do not stand at the foot of a face; never undercut one.

What this unlocks

With these skills you can find the raw materials for nearly every chapter in this part: Finding and Preparing Clay, Lime, Gypsum and Plaster of Paris, Portland Cement, Glass, Firebrick and Refractories and Abrasives and Grinding Stones. Good stone leads to Quarrying and Cutting Stone and Stone Masonry; metal-bearing stone leads to Finding and Identifying Ores and Mining and Tunnelling. Layers and fossils are also the beginning of the sciences of the earth and of life (The Scientific Method, Cells, Life and Evolution).

How it was first done

People have chosen stone carefully for at least 2.5 million years: the first stone-tool makers in East Africa already carried good fine-grained rock several kilometres to where they worked. Ochre — red hematite — was dug and ground for pigment more than 100,000 years ago. The ancient Greek writer Theophrastus (about 315 BC) wrote the first surviving book on stones, describing how they behave in fire. Georgius Agricola, a German doctor working in mining towns, described minerals by colour, lustre, hardness and taste in 1546. In the 18th century, James Hutton in Scotland realised that rocks are built up and worn down in endless slow cycles, and in 1815 William Smith, a canal surveyor, published the first geological map of a whole country, England and Wales — made by following rock layers and their fossils exactly as described in this chapter.