The clear, flexible plastic ribbon that carries a photographic emulsion. Why glass plates give way to film, why old nitrate film is too dangerous to keep, how cellulose acetate "safety film" is cast, subbed, coated, slit and spooled, and what a workshop can do before a chemical works exists.

Difficulty
●●●●●
Time
An afternoon to cast a few test sheets from acetate flake; a chemical works and months of tuning for continuous roll film
Steps from zero
28 prerequisites →

You need first

Early PlasticsPhotography

This unlocks

—

Raw materials

cottonsoftwood
The full path from nothing — 28 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Pottery
  10. The Kiln
  11. Charcoal
  12. Hides and Leather
  13. Lime
  14. Lye and Potash
  15. Fermentation
  16. Glass
  17. Bellows
  18. Saltpeter
  19. Distillation
  20. Copper Smelting
  21. Lead
  22. Sulfuric Acid
  23. Laboratory Glassware
  24. Lenses
  25. Gold and Silver
  26. Nitric Acid
  27. Early Plastics
  28. Photography
  29. Photographic Film Base

Do them roughly in this order. See it on the tech tree →

Why it matters

The gelatin dry plate of Photography gives superb negatives, but glass is heavy, fragile, bulky and one picture per plate. A box of a dozen 9 × 12 cm plates weighs about a kilogram. The same twelve pictures on roll film weigh a few grams and wind onto a spool the size of a thumb.

Film gives small cameras loaded in daylight, moving pictures (the only way to record motion before Cathode Rays and Television), a whole book on 3 metres of Microfilm and Document Storage, and X-Rays that do not shatter when dropped.

The difficulty is the base: the clear ribbon under the emulsion. It must be as clear as glass, tough, flexible, flat, unchanged by processing, and must not shrink, rot or catch fire in storage. Finding it took fifty years and three tries. This chapter tells you which to use, which never to make, and how film is cast and finished.

How it works

A finished film is a stack of thin layers. The base does nothing photographic; it is a carrier.

light from the lens Supercoat hard gelatin, about 1 µm Emulsion silver bromide in gelatin, 5–25 µm Sub layer glues gelatin to plastic Base clear acetate, 80–180 µm Backing anti-curl gelatin, dyed to stop halation Dashed orange: light that would bounce back off the base and make a halo. The dyed backing absorbs it. Not to scale: the base is really about ten times thicker than the emulsion.
Fig. 1 A sheet of film in cross-section, much enlarged. The emulsion sits on a thin gelatin sub layer that bonds it to the clear plastic base. A gelatin backing on the other side balances curl and stops light reflecting back into the emulsion.
Layer Thickness Job
Supercoat 1 µm Hard clear gelatin that protects against scratches
Emulsion 5–25 µm Silver bromide in gelatin: the picture (Photography)
Sub (substratum) under 1 µm Glues gelatin to plastic, which otherwise peels off
Base 80–180 µm Clear, tough, flexible carrier
Backing 5–10 µm Gelatin that balances curl; often dyed to stop halation

(1 µm is a thousandth of a millimetre. A human hair is about 70 µm.)

Why the backing matters. Gelatin shrinks as it dries, so film coated on one side curls into a tube. A gelatin layer on the back pulls equally the other way. Dyed with a dye that washes out in the developer, it also soaks up light that would bounce off the back of the base and make a halo round every bright point (halation).

The three bases. All three are long-chain molecules (Petrochemicals and Modern Plastics):

Base Made from Burns? Keeps Use
Cellulose nitrate Cotton + nitric acid Fiercely, and decays to a fire risk Decades, then decomposes Do not make. 1889–1951
Cellulose acetate ("safety") Cotton or wood pulp + acetic acid and acetic anhydride Slowly, like paper 40–50 years warm and damp; centuries cold and dry The base to make
Polyester Oil chemicals (Petrochemicals and Modern Plastics) Melts, slow Centuries Best, but needs a petrochemical industry

Cellulose, the chain of sugar units that makes cotton and wood, carries three hydroxyl groups (an oxygen with a hydrogen, the group that makes sugar love water) on each unit. Swap them for acetyl groups (the working part of acetic acid, the acid of vinegar) and you get cellulose acetate. It no longer swells much in water but dissolves in acetone. Pour the solution into a thin sheet, let the solvent evaporate, and a clear, tough film is left. That is the whole idea of a cast film base.

Nitrate film: why not

The first practical roll film, from 1889, was cellulose nitrate softened with camphor, which is celluloid. It was clear, tough and easy to cast, and almost all film made before about 1950 is nitrate. This book does not describe how to make it.

  • It burns faster than paper and supplies its own oxygen. A burning reel cannot be smothered; it can keep burning under water or under a blanket.
  • Its smoke kills. Burning or decomposing nitrate gives off nitrogen oxides and carbon monoxide. In the Cleveland Clinic fire of 1929, 123 people died, most of them from the gas of burning nitrate X-ray film stored in a basement.
  • It decomposes by itself, ever faster: the picture fades to amber; the film turns sticky with a sharp acid smell, then soft and bubbled, welded into a block, then an acrid brown powder. Decaying nitrate in a hot attic can catch fire spontaneously.

Danger If you find old film, treat it as nitrate until proved otherwise. Old cinema reels, X-ray films and negatives from before about 1950 are often nitrate. Keep them in metal cans, in small numbers, in a cool, ventilated outbuilding away from people, never in a house, office or library. Do not unwind badly decayed film. Copy anything valuable onto safety film or glass by contact printing, then destroy the nitrate a few strips at a time, outdoors, upwind, well away from buildings.

Telling nitrate from safety film. Look along the edge: makers printed SAFETY or NITRATE in the margin from about 1930. Otherwise, outdoors, on a stone, light a sliver no bigger than a rice grain cut from the margin:

  • Nitrate flares up at once with a bright yellow flame and is gone in a second, leaving almost nothing.
  • Acetate catches reluctantly, melts and drips, burns slowly, often goes out, and smells of vinegar.
  • Polyester shrivels, melts and barely burns, with a sweetish smoke. It is also almost impossible to tear.

What you need

Item Amount Notes
Cellulose acetate flake (acetone-soluble "secondary" acetate) About 18 g per 30 × 40 cm sheet From a chemical works (below)
Acetone About 120 ml per sheet Ether, Acetone and Solvents
Plasticiser 10–15% of the acetate weight From the works with the flake
Casting glass Flat plate glass, 40 × 50 cm or more Window Glass; the flattest you have
Spreader A straight bar with a 1 mm gap under it Brass or hardwood, below
Level and a heavy table Rules, Squares, Callipers and Gauges
Gelatin, chrome alum or formalin A few grams Sub and backing; Gelatin, Methanol and Formaldehyde
Emulsion As for plates Photography
Micrometer Reads 0.01 mm Rules, Squares, Callipers and Gauges
Sharp blades, a straightedge, a punch For slitting and perforating

Where to find it

Method 1: Before there is a chemical works

Honestly: until you can make or buy cellulose acetate, glass plates are the better choice for any picture you want to keep. But two flexible stopgaps are historically proven.

Waxed paper negatives. The calotype of Photography is already a flexible film: paper, made translucent with beeswax. Large, light and unbreakable, but grainy.

Stripping film. Emulsion is coated on paper over a layer of soluble gelatin; after processing, the emulsion is peeled off the paper onto a clear support.

  1. Brush smooth, well-sized paper with warm 2% gelatin in water, with no alum or hardener in it. Dry.
  2. Coat with dry-plate emulsion as for a glass plate, about 5 ml per 9 × 12 cm, and dry in the dark. It can be cut into strips and rolled on a spool; this is how the first Kodak camera of 1888 was loaded.
  3. Expose, develop, fix and wash as usual.
  4. Squeegee the wet negative face down onto a clean glass plate rubbed with a trace of wax. Soak the back with water at about 40 °C until the paper lifts; peel it away, leaving the emulsion on the glass.
  5. Pour over it a 10% gelatin solution containing a few drops of glycerine (from Soap making) and a pinch of chrome alum or a few drops of formalin to harden it, about 10 ml per 9 × 12 cm. Dry for a day, then peel the whole skin off the glass.

The result is a thin, flexible gelatin negative. It curls in damp air but prints well and weighs nothing. Expect to spoil a few at first.

Method 2: Cellulose acetate safety film

Making the acetate (works process, in outline)

This step belongs in a chemical works with acid-proof vessels, trained staff and solvent recovery. In outline:

  1. Purify the cellulose. Cotton linters or dissolving pulp are boiled in dilute Lye and Potash, lightly bleached, washed and dried thoroughly.
  2. Activate. The fluffed cellulose is soaked in strong acetic acid so the fibres open up and react evenly.
  3. Acetylate. In a cooled, stirred, acid-proof mixer, the cellulose is treated with acetic anhydride, a water-free relative of acetic acid made as a separate reagent in the works, in more acetic acid with a little Sulfuric Acid as a helper (a catalyst). The reaction must be kept cool, or the chains break and the film is weak. The fibres vanish into a clear syrup of fully acetylated cellulose (triacetate).
  4. Ripen. Water is added and the syrup held warm for many hours. Some acetyl groups come off again, giving secondary acetate, which dissolves in plain acetone. The works tests samples to stop at the right point.
  5. Precipitate and wash. The syrup is poured into dilute acid and water; the acetate falls out as white flakes, which are washed for a long time (acid left in them makes the film decay early) and dried.

Warning Acetic anhydride is a works reagent only. It reacts with water violently, its vapour severely burns the eyes and lungs, and splashes cause deep burns. This book does not describe making or handling it outside an industrial plant. Small workshops should obtain finished acetate flake and start at the next step.

Casting sheets by hand

With acetate flake, a workshop can cast flat sheets for sheet film, test pieces and short strips.

  1. Make the dope. In a stoppered glass jar, stir 15 g of acetone-soluble acetate flake and about 2 g plasticiser into 100 ml of acetone. A plasticiser is an oily liquid that stays inside the plastic and keeps it from going brittle. Leave it a day, shaking now and then, until it is a clear, honey-thick syrup with no lumps. Let it stand another day for bubbles to rise.
  2. Prepare the glass. Wash it with lye and chalk, rinse, dry, and polish with a clean cloth. Set it on a heavy table and level it in both directions. Stick two strips of metal foil or thin card 1 mm thick along the long edges as rails.
  3. Pour and spread. Pour the dope in a pool across one end. Draw the spreader bar along the rails in one smooth, steady stroke of about 5 seconds. The gap under it leaves a wet layer 1 mm thick.
  4. Dry slowly. Cover at once with a shallow box raised a few millimetres on blocks, so the acetone escapes gently. Fast drying in damp air chills the surface until water condenses on it, and the film dries milky (blush). Work on a dry day, or warm the glass a little.
  5. Strip. After 1–2 hours the film is firm. Slide the glass into a tray of water for a few minutes, lift a corner with a blade, and peel the film off slowly.
  6. Season. Hang the sheet in a drying cupboard at 50–60 °C, away from any flame, for a day or two. Solvent left inside makes the film shrink and curl for weeks afterwards.

A wet layer 1 mm thick gives a dry film about 0.1 mm thick, the thickness of roll film. For stiff sheet film, use a 1.5–2 mm gap and expect about 0.18 mm.

The casting wheel

Continuous film is cast the same way, but on a machine running day and night.

Filtered dope Slot hopper lays an even wet sheet Polished wheel, 2–6 m across turns once in several minutes Warm air solvent drawn off and recovered Film peeled off here (still slightly soft) Curing cabinet, 60–100 °C Master roll 1–1.4 m wide
Fig. 2 A film-casting machine. Dope runs from a slot hopper onto a large, slowly turning polished wheel. Warm air dries it as it travels most of the way round. It is peeled off as a continuous film, passes up and down over rollers in a long heated cabinet to drive out the last solvent, and is wound onto a roll.
  • The wheel (or an endless metal band), 2–6 m across, is polished to a mirror: every scratch is copied into every metre of film. Eastman's first works of 1889 cast onto glass tables about 60 m long.
  • Filtered, bubble-free dope is laid on through a slot hopper, a box with a long adjustable lip. Warm air drives off the solvent, which is recovered (Activated Charcoal, Distillation).
  • The film is peeled off still slightly soft, cured in a heated cabinet at 60–100 °C, and wound into a master roll 1–1.4 m wide.

Triacetate, the best acetate, does not dissolve in acetone; it is cast from methylene chloride with a little methanol, solvents only a works can make and recover. Hand casting uses secondary acetate and acetone.

Sub and backing

Gelatin will not stick to bare acetate.

  1. Sub. Dissolve about 0.5 g of gelatin in a few millilitres of water with a little strong acetic acid, then stir it into about 100 ml of acetone with a little alcohol. Brush or roll a very thin coat onto the base and dry. The solvent softens the plastic surface for a moment so the gelatin roots into it. Test the proportions on scraps: the sub must not make the base hazy.
  2. Backing. On the other side, coat a thin layer of 3–4% gelatin, hardened with a trace of chrome alum. For antihalation, dye it dark with a dye that the developer washes out.

Coating, slitting and spooling

Coating by hand. Stick a subbed sheet face up onto a level glass plate with a film of water under it (it clings flat), tape the edges, and coat it with emulsion exactly like a dry plate (Photography): about 5 ml per 9 × 12 cm, chilled on cold stone to set, dried for a day in a dark, dust-free box. Peel it off and trim.

Coating by machine. The base runs under a slot hopper of emulsion at 35–40 °C, through a chill section at about 10 °C where the gelatin sets, then hangs in long loops (festoons) in clean, conditioned air until dry. From here on, all work is in darkness or safelight.

Slitting. Pairs of circular knives, overlapping like scissors, cut the wide roll into ribbons. Dust must be sucked away: each speck on the emulsion prints as a white spot.

Format Width Notes
Sheet film 9 × 12 cm, 4 × 5 in and others Thicker base, 0.18 mm, fits a plate holder
Roll film (120) About 61–62 mm 12 frames 6 × 6 cm; paper-backed
35 mm 35 mm Perforated both edges, 4.75 mm pitch; 36 frames of 24 × 36 mm
Cine film 35 mm or 16 mm 4 perforations per 35 mm frame, 24 frames a second

Perforating. A punch-and-die block punches the edge holes, the film advanced by pins in the holes just punched so spacing stays accurate to a few hundredths of a millimetre (Presses, Punches and Dies). Otherwise the pictures jump on the screen.

Roll film and the spool

1234 leader 2 Flange about 25 mm Core with slot about 12 mm thick Key slot for the winding knob Red window in camera back Backing paper black inside, numbers outside Tape joint Film, about 61 mm wide emulsion facing away from the paper; 12 frames of 6 × 6 cm
Fig. 3 Roll film, exploded. The film is taped at one end to a longer strip of backing paper, black inside and printed with frame numbers outside. Both wind together onto a flanged spool. In the camera, the numbers are read through a small red window in the back.

Paper-backed roll film loads in daylight and needs no sprockets, so it is the easiest film camera to build.

  1. The spool. Turn a hardwood core about 12 mm thick and a little longer than the film is wide, with a lengthwise slot for the paper end (Wood Turning and Treen). Fit flanges about 25 mm across of thin tinplate or wood at each end, with a slotted key-hole at one end for the camera's winding knob (Tins, Cans, Drums and Tanks).
  2. The backing paper. Strong, smooth, opaque paper a millimetre wider than the film and longer by about a metre: black on the inside (dye it, or coat it with lampblack in shellac, then test that a lamp does not show through), with frame numbers printed large on the outside, spaced at the frame advance. Leave a long leader and a long tail.
  3. Load in darkness: lay the film on the paper, emulsion away from the paper, tape the leading end of the film to the paper, roll both tightly onto the spool, and seal the end with a gummed strip.
  4. The camera has a small window in its back covered with deep red glass or red-dyed film. The early plain emulsion of Photography is blind to red light, so the photographer can wind on until the next number appears without fogging the film. With red-sensitive film, keep the window covered and peek only briefly in shade.

How to tell it worked

  • Clarity. Laid on a printed page, good base is invisible. Hold it to a window: no haze, streaks, bubbles or specks.
  • Thickness. Measured with a micrometer at ten places, good film is within ±5%. Bands come from a wobbling spreader.
  • Flatness. A processed, dried strip lies flat or curls gently. A tight tube means too little backing.
  • Toughness. Folded right over and creased with a fingernail, acetate whitens at the crease but does not snap. Brittle film has too little plasticiser.
  • Dimensional stability. Mark two fine scratches 100 mm apart, soak the strip in water for 10 minutes, dry it, measure again. Good acetate changes by less than 0.5 mm.
  • Emulsion grip. After processing, press sticky tape on a corner of the emulsion and rip it off. The emulsion should stay. If it lifts, the sub is wrong.
  • Burn test of a sliver (above): slow and smelling of vinegar.

Note Troubleshooting. Milky, hazy film → blush: humid air or drying too fast. Dry slower, warmer, on a dry day; add a little higher-boiling solvent if the works supplies one. Orange-peel or rippled surface → draughts during drying, or dope too thin. Cover the casting. Bubbles and pinholes → dope not rested; stir gently, let it stand longer. Film shrinks and curls for weeks → solvent left in it. Season longer and warmer. Emulsion peels off in the developer → no sub, or sub too weak; also keep processing baths below 22 °C. Yellow, brittle film that smells of vinegar → acid left in the flake. The works must wash it longer.

Dangers

Danger Acetone and other film solvents are highly flammable, and their vapour is heavier than air, flowing along floors to a flame metres away. Cast film only with no flame, stove or spark in the room, in a through-draught. The vapour also causes headache and dizziness.

  • Nitrate film (above): never make it, never store it near people.
  • Acetic anhydride, methylene chloride and strong acids belong only in a works with fume extraction and trained staff.
  • Vinegar syndrome. Decaying acetate gives off acetic acid, which speeds the decay of everything stored with it. Keep a strip of indicator paper (pH, Indicators and Buffers) in film cans and check it each year: a colour change means the film is starting to go. Copy it while it is still sound.

Storage. Acetate kept at room temperature and moderate humidity usually begins to decay after about 40–50 years. Kept cold (a cellar or cold store) and dry (30–40% relative humidity, Rain Gauges, Anemometers and Weather Stations), it lasts many times longer. Store film in cans or boxes that let acid vapour escape, away from paint, fresh wood and cardboard.

What this unlocks

Film makes the hand camera, aerial survey for Maps and Mapmaking, long rolls of Microfilm and Document Storage for Libraries and Preserving Knowledge, unbreakable X-Rays, and cinema, with a sound track printed beside the pictures (Recording Sound). The casting machine also makes clear packaging film and the base of magnetic recording tape.

The best base of all is polyester (Petrochemicals and Modern Plastics): stronger, more stable and longer-lived than acetate, made by stretching a melted sheet in two directions, and needing the whole petrochemical industry. For records meant to last centuries, use glass plates or polyester.

How it was first done

In 1884–85 George Eastman of Rochester, New York, sold paper roll film and, with William Walker, a roll holder that fitted plate cameras; his stripping film, with the emulsion peeled off the paper after processing, loaded the first Kodak camera of 1888. The clergyman Hannibal Goodwin of Newark, New Jersey, applied in 1887 for a patent on transparent nitrocellulose film; Eastman's chemist Henry Reichenbach patented a similar method, and Eastman sold transparent nitrate roll film from 1889. Goodwin's patent was finally granted in 1898, and in 1913–14 the courts found that Eastman had infringed it. John Carbutt in Philadelphia sold celluloid sheet film from 1888.

Cellulose acetate was first made by Paul Schützenberger in France in 1865. Acetone-soluble acetate was found by George Miles in the United States and by Arthur Eichengrün and Theodore Becker at Bayer in Germany around 1903–05. Kodak sold acetate safety film from about 1909, and its 16 mm home-movie film of 1923 was made only on safety base. Nitrate remained standard for 35 mm cinema film until cellulose triacetate, introduced by Kodak in 1948, finally matched it; Kodak stopped making nitrate film in 1951. Kodak introduced polyester film base under the name Estar in 1955.