◆ Rebuild

Part 8 · Chemistry

Separating the Rare Earths

The rare earths, fifteen lanthanide metals with yttrium beside them, are so alike that they ride together through every ordinary chemical step. Splitting them one from another takes patience multiplied by many small steps. Fractional crystallisation does it in dishes over months. A cascade of mixer-settlers does it with solvent and acid, stage after stage, around the clock. A column of ion-exchange beads sorts a mixture into neat bands of pure metal. With these you get the neodymium and samarium for strong magnets and the europium and yttrium that make the red of colour screens.

Difficulty
●●●●●
Time
Months of evenings for fractional crystallisation; a cascade runs continuously for weeks before it settles down; an ion-exchange run takes one to four weeks
Steps from zero
38 prerequisites →

You need first

Rare Earths, Cerium and PhosphorsWater Softening and Ion Exchange

This unlocks

—
The full path from nothing — 38 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Measurement from Scratch
  8. Writing and Numbers
  9. Hunting and Trapping
  10. Basic Woodworking
  11. Pottery
  12. The Kiln
  13. Charcoal
  14. Arithmetic and Fractions
  15. Hides and Leather
  16. Lime
  17. Tiles and Clay Pipes
  18. Salt
  19. Surveying and Levelling
  20. Lye and Potash
  21. Fermentation
  22. Glass
  23. Bellows
  24. Acids, Bases and Testing
  25. Saltpeter
  26. Lead
  27. Copper Smelting
  28. Laboratory Glassware
  29. Sulfuric Acid
  30. Pipes, Plumbing and Aqueducts
  31. Identifying Substances
  32. Nitric Acid
  33. The Battery
  34. Rare Earths, Cerium and Phosphors
  35. Electrolysis
  36. Chlorine and Bleach
  37. Water Treatment for a Town
  38. Water Softening and Ion Exchange
  39. Separating the Rare Earths

Do them roughly in this order. See it on the tech tree →

Why it matters

Rare Earths, Cerium and Phosphors shows how to crack monazite and split it into a few broad groups: cerium, a light group, and a yttrium group. That gives flints, mantles and polishing powder. It does not give single elements, and several of the most valuable modern things need exactly one of them:

Element What it makes How pure
Neodymium (with praseodymium) Neodymium–iron–boron magnets: the strongest there are, for motors, generators, loudspeakers and hard disks (Permanent Magnets, The Electric Motor, Wind Turbines) 95–99 %; praseodymium may stay in
Samarium Samarium–cobalt magnets, which keep their strength up to 300 °C 99 %
Europium The red phosphor of colour television, flat screens and three-colour lamps (Cathode Rays and Television, Flat Screens: LCD and LED Displays, Arc Lamps, Neon and Fluorescent Lights) 99.9 % or better
Yttrium The host crystal for that red phosphor; lasers; tough zirconia (Zircon and Zirconium) 99.99 % for phosphors
Terbium, dysprosium Green phosphor; a few percent of dysprosium keeps neodymium magnets strong when hot 99 %+
Lanthanum Optical glass with a high refractive index (Optical Glass and Achromatic Lenses), hydrogen-storing alloys 99 %

Be realistic: this is among the hardest chemistry in the book. Each step is simple, but there are hundreds of them, and the best methods need factory-made organic chemicals. Plan for a dedicated works, not a weekend.

How it works

Why they are so hard to part

All the rare earths form ions with a charge of three, and their size shrinks by only about one percent from each element to the next. In any one step, one neighbour goes only slightly more one way than the other.

That difference is the separation factor, β (beta). If a solvent takes 1.5 times as large a share of neodymium as of praseodymium, β is 1.5. One shake enriches the mixture only a little, but many in a row multiply: ten stages at β = 1.5 give a factor of about 58, twenty give over 3,000.

Pair Typical β (acidic extractant) Stages for 99 % purity, roughly
Lanthanum / cerium 3 15–20
Praseodymium / neodymium 1.4–1.5 60–100
Neodymium / samarium 8–10 10
Samarium / europium 2 25–35
Europium / gadolinium 1.5 50–70

Praseodymium and neodymium are the hardest common pair. Luckily, magnets work almost as well with the mixture, called didymium. Leave the pair together unless you need one alone.

Short cuts first

Two elements can be pulled out by changing their charge, which no amount of stage work can match:

  • Cerium goes to a charge of four when oxidised and then falls out as a yellow solid. Rare Earths, Cerium and Phosphors shows how. Removing it first takes away half the bulk.
  • Europium goes to a charge of two when reduced with zinc and then falls out with sulfate, like barium. Rare Earths, Cerium and Phosphors gives McCoy's method. Done on a fraction already rich in europium, it gives 99.9 % in a few cycles.

Everything else has to be done by one of the three methods below.

Mixed rare earthsthorium already removed oxidise; weak acid Ceriumyellow solid: polish, flints La, Pr, Nd, Sm, Eu, Gd … Ychloride solution cascade 1 Lanthanumleaves in the water: optical glass Pr, Nd, Sm, Eu, Gd … Ystripped from the solvent cascade 2 Didymium (Pr + Nd)neodymium–iron–boron magnets Sm, Eu, Gd + yttrium groupa few percent of the start cascade 3 Samariumsamarium–cobalt magnets Eu, Gd + yttrium groupeuropium now well enriched ion-exchange columns zinc Europiumreduced, falls as sulfate: red phosphor Bands from the columnone element per fraction Yttrium, terbium, dysprosiumphosphors, lasers, hot magnets Every product: oxalic acid → oxalate → burn at 850–900 °C → oxidecheck each one with the spectroscope and a radiation counter
Fig. 1 The path from monazite to separate rare earths. Cerium and europium are taken out by changing their charge. The remaining mixture is split by solvent extraction: lanthanum first, then didymium for magnets, then samarium, then the yttrium group. Each pure solution ends as oxalate, burned to oxide.

What you need

Item Use See
Mixed rare-earth hydroxide or chloride, thorium removed Starting material Rare Earths, Cerium and Phosphors
Hydrochloric Acid, Nitric Acid Dissolving, scrubbing, stripping
Ammonia or caustic soda (Lye and Potash) Adjusting acidity; "saponifying" the extractant
Oxalic acid Bringing each product down Oxalic Acid
Kerosene (lamp paraffin) Carrier for the extractant Petroleum and Refining
Extractant: tributyl phosphate or an organophosphoric acid The chemical that grabs rare earths Organic Synthesis and Fine Chemicals
Cation-exchange resin beads, fine For columns Water Softening and Ion Exchange
Citric acid or EDTA Eluting the columns Citric and Tartaric Acid
A The Spectroscope Following neodymium, praseodymium and others by their absorption lines
Glass, glazed stoneware, polythene or fibreglass vessels Acid-proof, solvent-proof plant Laboratory Glassware, Petrochemicals and Modern Plastics, Composites: Fibreglass, Carbon Fibre and Honeycomb
A radiation counter Checking for thorium and radium

Where to find it

The ores are monazite, bastnaesite and xenotime: see Rare Earths, Cerium and Phosphors. Xenotime is worth seeking because it is rich in yttrium and the heavy group (dysprosium, terbium), which monazite has little of. In monazite the light rare earths dominate: roughly cerium 45 %, lanthanum 23 %, neodymium 18 %, praseodymium 5 %, samarium 3 %, and europium only about 0.1 %. Expect only 0.5–1 g of europium oxide from 1 kg of mixed oxide.

Method 1: Fractional crystallisation

This needs only dishes, heat and patience. It is how every rare earth was first isolated. Use it to learn, to make small amounts, or when you have no extractant.

The salt. For the light group, use the double ammonium nitrates. Dissolve the mixed oxides (cerium removed) in nitric acid and add ammonium nitrate equal to about 1.5 times the weight of oxide. For the middle group (samarium, europium, gadolinium), use double magnesium nitrates in the same way, with magnesium nitrate. Lanthanum's double salt is the least soluble, then praseodymium's, then neodymium's.

The triangle scheme.

  1. Dissolve the salt in the least hot water (with a few drops of nitric acid) that will hold it at about 80 °C. Let it cool overnight. Crystals form.
  2. Pour off the liquid. You now have crystals (C), a little richer in lanthanum, and liquor (L), a little richer in neodymium.
  3. Redissolve C with fresh hot water and crystallise again: it splits into C₁ and L₁. Boil L down and crystallise: it splits into C₂ and L₂.
  4. Now combine L₁ with C₂ (they are about the same composition) and recrystallise that. Each round you add one more dish to the row, always combining the liquor from one dish with the crystals from its neighbour.
  5. After 10–20 rounds, the row of dishes runs from nearly pure lanthanum at the "crystal" end through praseodymium (green) to neodymium (lilac) at the "liquor" end.

Following it by colour. Praseodymium salts are leek green. Neodymium salts are lilac to rose. Lanthanum's are colourless. Better, look at a strong solution through the The Spectroscope against a bright lamp. Neodymium shows sharp dark lines in the yellow (around 575–580 nm) and green. Praseodymium shows a group of lines in the blue (about 445–480 nm). As the lines of one fade from a dish, that end is getting purer.

Keep a dish-by-dish log; a mix-up wastes weeks. Reaching 99 % on any pair takes hundreds of crystallisations. The extraction cascade below does the same thing automatically.

Method 2: Solvent extraction in mixer-settlers

This is how nearly all rare earths are separated today. It runs continuously and scales from a bench to a factory.

The principle

Water and kerosene do not mix. Dissolve an extractant in the kerosene: a chemical with an oily tail and an end that grips metal ions. Shake it with a rare-earth solution in water, and some of each rare earth moves into the kerosene, the heavier ones a little more readily.

The ratio of an element in the kerosene to that in the water is its distribution ratio, D. More acid in the water pushes rare earths back into the water. That gives three operations:

  • Extraction: low acid. The rare earths go into the solvent, the heavier ones preferentially.
  • Scrubbing: moderately acid water washes the lighter ones back out of the solvent, so the solvent holds mostly the heavier ones.
  • Stripping: strong acid (about 4–6 mol/L hydrochloric acid) pulls everything back into water, freeing the solvent for reuse.

The extractants

Extractant Use Notes
TBP (tributyl phosphate) From strong nitrate solutions The first one used, in the 1950s. From butanol (Fermentation) and phosphorus oxychloride (Phosphorus, Chlorine and Bleach). Used 30–100 % in kerosene
D2EHPA (an organophosphoric acid) From dilute chloride solution Strong; separates the middle and heavy group well
P507 (an organophosphonic acid) From chloride solution The modern workhorse for the light group, including praseodymium and neodymium

All three are made in a fine-chemical works (Organic Synthesis and Fine Chemicals). The acidic types are "saponified" before use: shaken with ammonia or lye to turn about a third of them into their ammonium or sodium salt. This stops the water from becoming too acid as metal is taken up. Typical solvent: 1–1.5 mol/L of extractant in kerosene, with a little long-chain alcohol to stop a third, sticky layer forming.

Measuring D in a funnel

Before building any plant, shake equal volumes of solvent and feed in a separatory funnel for 5 minutes. Separate them, strip the solvent with strong acid, and precipitate, burn and weigh the oxide from each. D = oxide from solvent ÷ oxide from water. The spectroscope shows how the neodymium-to-praseodymium ratio changed. Repeat at three or four acidities to choose your plant's acids.

The mixer-settler

One stage, cut open from the side Motor solvent in water in solvent out water out Mixerpaddle, 2–5 minutes Baffleopen at the bottom Settler4 times the mixer's areasolvent (light) floats water (heavy) sinksinterface Top weirsolvent spills overDamwater passes under Weirslides upand downto set theinterface A cascade: stages in a row, solvent one way, water the other Extraction Scrubbing Stripping solvent → clean solvent returns to the start Feed Scrub acid Strong acid Light ones out(raffinate) Heavy ones out
Fig. 2 Above: one mixer-settler stage in cross-section. A paddle mixes solvent and water; the mixture flows into a long, quiet settler, where the light solvent floats and spills over the top weir one way, and the heavy water passes under a dam and over an adjustable weir the other way. Below: a cascade of such stages in three sections. Solvent and water flow in opposite directions; the light rare earths leave in the water at one end, and the heavy ones are stripped out of the solvent at the other.

A mixer-settler is one stage: a box with a small mixing chamber and a long settling chamber.

Solvent from the stage on one side and water from the stage on the other enter the mixer. A paddle or turbine stirs them into a cloudy emulsion for 2–5 minutes while metal moves between them. The emulsion passes a baffle into the still settler, where the drops join up: solvent on top, water below. The solvent spills over a top weir to the next stage one way; the water flows under a dam and over an adjustable weir to the next stage the other way. That weir sets the height of the interface between the two layers; keep it about mid-depth.

Sizes for a bench cascade (a few kilograms of oxide a month):

Part Size
Mixing chamber 6 × 6 cm, 8 cm deep: about 0.25 litre
Settler 6 cm wide, 25–30 cm long, same depth
Impeller A flat paddle or disc turbine 3–4 cm across, 300–600 turns a minute
Flow Each liquid 1–3 litres an hour
Number of stages 20–40 for didymium; 60–100 to split praseodymium from neodymium

A settler should be about four times the area of the mixer. If drops are still cloudy at the far end, it is too small or the flow is too fast.

Sizes for a works: mixers of 0.2–2 m³, settlers of 2–10 m², rows of 50–100 stages or more.

How to make one.

  1. Small: glue sheets of clear polythene, PVC or acrylic into a long box with partitions (Petrochemicals and Modern Plastics). Glass is fine for a few stages. Plywood boxes lined with fibreglass in polyester or vinyl-ester resin last for years (Composites: Fibreglass, Carbon Fibre and Honeycomb). Do not use bare metal: the acid eats iron, and even a trace of iron spoils the products.
  2. Make a row of identical stages sharing walls. Number each one.
  3. Drive the impellers from one line shaft above the row by small belts, or give each its own small motor (The Electric Motor). Use glass, polythene or stainless shafts.
  4. Make each water weir a slotted plate that slides up and down, or a short tube that can be turned.
  5. Feed solvent and water from head tanks through glass tubes with clamps or needle valves, with a flow meter or a measured cup and watch.
  6. Fit a lid. Kerosene smells and burns, and dust spoils settling.

Running a cascade

A real separation has three sections in one long row:

  1. Extraction section (say 15–25 stages). Feed solution, about 1 mol/L rare-earth chloride at pH 2–3, enters at the joint between extraction and scrub sections. Solvent flows one way, water the other. The heavier element follows the solvent; the lighter one stays in the water and leaves as the raffinate at the end.
  2. Scrubbing section (15–40 stages). Dilute acid flows against the loaded solvent and pushes the lighter element back down towards the feed point.
  3. Stripping section (5–8 stages). Strong hydrochloric acid takes the heavier element out of the solvent. The solvent goes back to the start.

Every split is one more cascade, or one more pass through the same one with new settings: lanthanum from didymium, then didymium from samarium, and so on.

Starting up. Fill every stage with solvent and water, start the impellers, and run with no feed for an hour to check the levels. Then start the feed. A cascade takes days to weeks to reach steady composition. Sample the outlets daily, precipitate the oxalates, and check them in the spectroscope. Adjust the scrub acid flow: more scrub gives a purer heavy product but more of it is pushed back into the light one.

From solution to oxide

From each product stream, precipitate with oxalic acid (about 1.2 times the weight of the oxide expected), filter, wash and burn the oxalate at 850–900 °C (orange heat) for two hours. Neodymium oxide is pale lilac-blue. Samarium oxide is creamy yellow. Europium oxide is white with a pink tinge. Yttrium oxide is pure white.

Method 3: Ion-exchange columns

Use columns for small amounts of very pure elements: europium and yttrium for phosphors, terbium, dysprosium, and laboratory standards.

The principle

Load a band of mixed rare earths on top of a tall column of cation-exchange beads (Water Softening and Ion Exchange), then push through a complexing agent: a chemical that wraps round rare-earth ions and drags them off the beads. Heavier rare earths are wrapped more tightly and move faster. Over a metre or more, the band sorts itself into touching bands, each one element, which come out of the bottom one after another. This is a form of Chromatography.

The separation column

41424344 Bands move down1–2 cm an hourcolumn 1–1.5 m tall,2.5–5 cm across Constant-level bottleammonium EDTA, pH 8.4 Beads already passedammonium form, empty of rare earths lanthanum (lightest, at the back) praseodymium (green) neodymium samarium, europium heavier ones, in front Copper retaining bedbright blue; the boundary showswhere the front has reached Glass wool on a perforated disc Tapinto numbered fraction bottles Touching bands,one element each
Fig. 3 An ion-exchange separation column. A band of mixed rare earths, pushed down by a complexing solution, sorts itself into touching bands of single elements, heaviest in front. A blue band of copper held on the beads ahead of it shows where the front is. Fractions are collected at the bottom and tested one by one.

Build:

  1. Tube: glass, 2.5–5 cm inside, 1–1.5 m long (Scientific Glassblowing and Glass-to-Metal Seals). For larger work, run several in series. Ames Laboratory used columns up to 75 cm across.
  2. Bottom: a plug of glass wool on a perforated glass disc, then a tap or a rubber tube with a screw clamp.
  3. Fill: pour in a thin slurry of the finest cation resin you have, 0.1–0.3 mm beads (sieve them), so it settles evenly with no air. Tap the tube as it settles. Fine beads give sharper bands but run more slowly.
  4. Top: a disc of filter paper or a layer of glass wool so incoming liquid does not stir the bed. Feed from a constant-level bottle (a Mariotte bottle: a sealed bottle with an air tube dipping into it) so the head stays steady day and night.

Using citrate (the simplest). Citric acid comes from lemons, limes or mould fermentation (Citric and Tartaric Acid).

  1. Load the rare-earth chloride on the top tenth of the bed.
  2. Elute with 5 % citric acid adjusted with ammonia to pH 2.5–3.5, at about 1 cm of column a minute.
  3. Collect fractions of 50–100 ml in numbered bottles. Precipitate a test drop from each with oxalic acid.

Citrate works but spreads the bands, so the fractions overlap. Use it for one element in high concentration, such as yttrium from a xenotime concentrate.

Using EDTA (much better). EDTA is a factory-made complexing agent (Organic Synthesis and Fine Chemicals). It gives sharp, touching bands.

  1. Convert the lower two-thirds of the column (or the second and third column in a series) to the copper form by running copper sulfate solution through it, then rinse. It turns bright blue. This "retaining bed" is needed because EDTA itself would crystallise in the column if the beads freed acid.
  2. Load the rare earths on the top third.
  3. Elute with 0.015 mol/L ammonium EDTA at pH 8.4.
  4. The front of the rare-earth bands pushes the copper ahead of it. You can watch the blue boundary move down the tube, a centimetre or two an hour.
  5. Copper EDTA comes out first, deep blue. Then the rare earths, heaviest first: lutetium, ytterbium … dysprosium, terbium, gadolinium, europium, samarium, neodymium, praseodymium, lanthanum. Yttrium comes out between dysprosium and terbium.

The middle of each band is commonly 99.9 % or better after one pass. The overlaps at the joints go back into the next run.

Get the rare earths back: acidify each fraction with hydrochloric acid to pH 1–2; the EDTA crystallises out and is reused. Precipitate the rare earth with oxalic acid.

Good and bad columns. A good column has flat, level band edges. Slanted or ragged edges mean the bed was packed unevenly or has air in it; repack it. A bed that cracks has been allowed to run dry: never let the liquid fall below the top of the beads.

Making the metals, in outline

  • Neodymium and didymium: electrolyse the oxide dissolved in molten neodymium and lithium fluorides at about 1,050 °C, carbon anode, tungsten cathode, much like the Aluminium cell (Electrolysis, Fluorspar and Fluorine Compounds).
  • Samarium: heat the oxide with lanthanum metal in a vacuum at 1,300–1,500 °C; samarium boils off as metal (High-Vacuum Pumps and Gauges). Or heat samarium oxide, cobalt powder and calcium at about 1,100 °C under argon and wash out the lime: the powder left is already samarium–cobalt magnet alloy (Permanent Magnets).
  • Europium and yttrium stay as oxides for phosphors.

How to tell it worked

  • Spectroscope: a strong solution of pure neodymium shows its yellow lines and none of praseodymium's blue ones, and the reverse.
  • Colour of the oxide: neodymium pale lilac-blue; praseodymium (as its black oxide) dark brown-black; lanthanum, yttrium and gadolinium pure white. A brown cast in "neodymium" oxide means praseodymium is still in it.
  • Europium: under an ultraviolet lamp, yttrium oxide fired with a pinch of your europium glows a sharp red. Iron or terbium dulls or shifts it.
  • Weight balance: the oxide from all outlets should match the oxide fed in, within a few percent.
  • Thorium out: the counter reads background near every product.

Note Troubleshooting. A thick, creamy third layer between solvent and water ("crud") → fine silica, iron or dust in the feed. Filter the feed and add 5 % of a long-chain alcohol to the solvent. Settlers flood with cloudy liquid → impellers too fast or flow too high. Slow them; settlers need four times the mixer area. Product purity drifts → a flow has changed. Check every flow daily. Column bands blur → flow too fast, beads too coarse, or an uneven bed. Halve the flow before anything else. White crystals block the column → EDTA acid crystallising. The retaining bed was too short or the pH too low.

Dangers

Danger Radioactivity. Thorium and its daughter radium follow the rare earths unless removed at the start (Rare Earths, Cerium and Phosphors). Radium also concentrates in scale on plant walls and in crud. Check every product and waste with a counter. Store residues wet, sealed and buried away from water. Never send raffinates into a stream (Detecting Radiation).

Danger Kerosene fires. A cascade holds tens to thousands of litres of kerosene, stirred by motors. Keep naked flames and sparking switches out of the hall, ventilate it, keep sand and foam ready (Fire Extinguishers and Alarms), and put each row in a bunded tray that can hold its whole contents.

  • Acids, ammonia and extractants burn or irritate skin and eyes; wear goggles and gloves (Acids, Bases and Testing).
  • Oxalic acid is a kidney poison (Oxalic Acid). Fluoride melts give off fumes that burn lungs and bones (Fluorspar and Fluorine Compounds).
  • Fine neodymium and samarium powders catch fire in air. Handle them under oil or inert gas.

What this unlocks

Strong, light electric motors and generators (The Electric Motor, Wind Turbines, Electric Vehicles); small loudspeakers and headphones (Loudspeakers, Microphones and Headphones); hard disks (Displays, Printers and Data Storage); red and green phosphors for Cathode Rays and Television, Flat Screens: LCD and LED Displays and efficient lamps; yttrium for Lasers; lanthanum glass for good camera Lenses. The same mixer-settlers separate nickel from cobalt (Nickel and Cobalt), purify uranium (Nuclear Energy (Overview)), and recover copper from weak leach solutions (Copper Smelting, Leaching, Solvent Extraction and Electrowinning).

How it was first done

Carl Auer von Welsbach separated praseodymium and neodymium in 1885 by about a hundred crystallisations of double ammonium nitrates. Eugène Demarçay found europium in 1901 with double magnesium nitrates. In 1947, working from the Manhattan Project, Frank Spedding and Jack Powell at Ames, Iowa, and teams at Oak Ridge, separated rare earths on ion-exchange columns, first with citrate and from the 1950s with EDTA, making kilograms of pure metals. Donald Peppard at Argonne showed in 1957 that organophosphoric acids extract rare earths strongly. Molycorp at Mountain Pass, California, began extracting europium for colour television in 1965. In China in the 1970s, Xu Guangxian worked out the theory of counter-current cascades that made the country the world's supplier. Karl Strnat found samarium–cobalt magnets in 1966–67, and Masato Sagawa at Sumitomo and John Croat at General Motors announced neodymium–iron–boron magnets in 1984.

Source: content/entries/chemistry/rare-earth-separation.md