◆ Rebuild

Part 6 · Building

Stone Masonry

How to build walls of stone that stand for centuries — dry stone field walls with no mortar at all, rubble walls bedded in lime, and squared ashlar — with the rules of bonding, through-stones, plumb and level, and how to span an opening with a stone lintel.

Difficulty
●●●●●
Time
A beginner builds a metre or two of field wall a day; a stone house takes a team a season
Steps from zero
8 prerequisites →

You need first

Quarrying and Cutting StoneMortar and Concrete

This unlocks

Dams and ReservoirsBuilding Against Earthquakes and StormsFoundations and FloorsWalls, Palisades and WatchtowersWells and CisternsCanals and LocksHarbours and Lighthouses
The full path from nothing — 8 steps before this one
  1. Stone Tools
  2. Fire
  3. Finding and Preparing Clay
  4. Simple Machines
  5. Quarrying and Cutting Stone
  6. The Kiln
  7. Lime
  8. Mortar and Concrete
  9. Stone Masonry

Do them roughly in this order. See it on the tech tree →

Why it matters

Stone does not rot, does not burn, and does not care about rain. A well-built stone wall can outlast every other thing you make. Dry stone field walls fence animals and terrace hillsides for farming (Farming from Seed); stone walls make houses, granaries (Granaries and Food Storage), wells (Wells and Cisterns), bridges (Roads and Bridges), mills, furnaces and harbours. Clearing stones from a field to build its wall improves the field at the same time.

Stone is heavy and slow to work, but you do not need to cut it perfectly: most of the stone buildings in the world are made of rough stones skilfully fitted. The secret is not the shape of the stones but how they are bonded — how each stone crosses the joints below it and ties the wall together.

How it works

  • Stone is very strong in compression (squeezing) and weak in tension (pulling) and bending. A wall standing upright is pure compression — stone's best case. A stone beam across a gap bends and cracks easily. That is why openings in stone walls are short, or arched (Arches, Vaults and Domes).
  • Walls fail by splitting, not crushing. A wall of stones simply piled up separates into two thin skins that bulge and fall. Bonding prevents this: stones that cross joints (each stone sits across the joint between two below it) and through-stones that reach from one face to the other lock the whole mass into one.
  • Gravity is your friend if the wall leans in. A wall that narrows as it rises (a batter) is far more stable than a vertical one, because its weight always falls inside its base.
  • Water and frost are the enemies. Water seeping into joints and cracks freezes, expands by about 9%, and pries stones apart. Shed water off every top surface, and use stone that does not soak it up.

What you need

Tool Use Notes
Walling hammer Trimming and knocking off corners 1.5–2 kg, a square face and a chisel end. See Blacksmithing
Lump hammer and chisels Shaping and dressing Pitching tool, point, claw and flat chisels with hardened Steel edges
Crowbar and levers Moving and placing heavy stones A 1.5 m iron bar, or a stout hardwood pole
Trowel, mortar board Mortared work Wood or iron
Plumb line, level, square Keeping it true See Measurement from Scratch
String lines and pegs Marking each course Strong, non-stretchy cord (Cordage and Rope)
Batter frames Guiding a sloping wall Two wooden frames the shape of the wall's cross-section

Stone weighs about 2.5 tonnes per cubic metre (granite 2.7, sandstone 2.3). A dry stone field wall 1.4 m high uses over a tonne of stone per metre of length. A house uses hundreds of tonnes. Build near your source; see Quarrying and Cutting Stone for getting it out of the ground, and Cranes and Lifting and Simple Machines for moving it.

Mortar for mortared work: lime mortar, 1 part lime putty to 3 parts sharp sand (Lime, Mortar and Concrete).

Choosing stone

  • Field stone — loose stones from fields, river banks and scree slopes. Free, already weathered (so what remains is the durable part), and good for rubble and dry walls. Flat, slabby stones are far easier to build with than round ones; round river cobbles are the hardest of all.
  • Limestone and sandstone — split along their beds (the layers the rock was laid down in) into flat slabs, and are easy to shape. Some are soft and weather away; test them.
  • Granite and other hard igneous rocks — extremely durable but very hard to shape.
  • Slate — splits into thin sheets; good for walls, lintels, damp-proof courses (Foundations and Floors) and roofs (Roofs).

Tests for good building stone:

  1. Ring test. Tap it with a hammer. Sound stone rings; a dull thud means hidden cracks or soft layers.
  2. Water test. Weigh a dry piece, soak it for a day, weigh again. A gain of more than about 5–6% of its weight means a thirsty stone that frost may destroy.
  3. Look at old exposures. Stone that has stood in an outcrop, old wall or gravestone for a century with sharp edges is good. Stone that has crumbled, flaked or rounded is not.
  4. Frost test. Soak samples and freeze them outdoors a dozen times over a winter. Discard any that crack or flake.

The rules of bonding

These rules apply to every kind of stone wall.

GOOD: JOINTS CROSSED BAD: RUNNING JOINTS Quoinslong and short, alternating Through-stones(dark) ends showing in the face every stone sits across a joint below Running jointa straight crack from top to bottom
Fig. 1 Bonding seen on the face of a wall. Good: every stone crosses a joint below it, long stones run into the wall, through-stones tie the faces together, and big quoins lock the corner. Bad: joints run straight up and the wall will split.
  1. One over two, two over one. Every stone should sit across the joint between two stones below it. Never let vertical joints line up from course to course — a running joint is a crack waiting to happen.
  2. Length into the wall. Lay each stone with its long side running into the wall, not along its face. It is tempting to put long stones along the face — it looks good and covers more wall — but they make a thin, weak skin.
  3. Lay it on its bed. Lay layered stone (limestone, sandstone, slate) with its layers horizontal, as it lay in the ground. On edge, frost splits the layers off.
  4. Solid on two points. Each stone must sit without rocking. If it rocks, wedge it from the inside of the wall with small stones (pinning), never from the face, where wedges get knocked out.
  5. Through-stones. At least one stone reaching right through the wall for every square metre of face, staggered.
  6. Corners (quoins) are built of the biggest, squarest stones, laid alternately along one face and then the other, so the corner is tied both ways.
  7. Shed water. Set stones level or tilting very slightly downward to the outside, so rain runs out, not in.

Method 1: The dry stone wall

A dry stone wall has no mortar at all. Its two faces lean together, and the weight of the stones holds them in place. A good one lasts 100–200 years with little care.

Cope stoneson edge, tight together String lineone for each face, raised as you go Heartingsmall stones placed by hand Through-stoneevery metre, at half height Battereach face leans in 1 cm per 6–8 cm Face stoneslong side into the wall Foundationbiggest stones, on firm subsoil 1.2–1.5 mhigh Batter frame(dashed) at each end 30–40 cm 60–90 cm
Fig. 2 A dry stone field wall in cross-section. Two battered faces of stones laid length-in, a core of packed hearting, a through-stone halfway up, and a row of cope stones on top. Batter frames and string lines guide the faces.

Typical size: 1.2–1.5 m high, 60–90 cm wide at the base, 30–40 cm wide under the coping. Each face leans inward about 1 cm for every 6–8 cm of height.

  1. Sort the stone. Spread it out along both sides of the line of the wall: big flat ones for the foundation, long ones for throughs, flat and wedge-shaped ones for the faces, small rubble for hearting, and the squarest for the copes. Sorting first saves hours of hunting.
  2. Mark and dig. Peg a string line on each side. Strip the turf and topsoil down to firm subsoil, 15–30 cm, in a trench 10 cm wider than the base on each side.
  3. Set up batter frames. Make two light wooden frames the exact shape of the wall's cross-section and stand one at each end of the length you will build, plumbed and braced. Stretch string lines between them, one for each face, and raise the lines as the wall grows.
  4. Foundation. Lay the biggest stones in the trench in two rows, length into the wall, with their flattest face up. Pack the gap between them with hearting.
  5. Build the faces. Lay stones along both faces, each touching the line with its face, crossing the joints below. Work both sides together, course by course.
  6. Hearting. Fill the middle as you go, course by course, with small stones placed by hand and packed tight — not shovelled or thrown in. Loose hearting is why walls bulge.
  7. Through-stones at about half height, every 0.9–1 m along the wall, reaching through both faces. Bring the wall up level first so they sit flat.
  8. Cope it. Finish with a row of stones set on edge across the top, tight against each other, as wide as the wall top. They protect the wall and their weight locks the top courses.

A beginner builds 1–2 m of wall a day; an experienced waller twice that or more.

Method 2: Mortared rubble walls

Rubble means rough or roughly shaped stones. Bedded in lime mortar, rubble makes the walls of most stone houses.

  1. Foundations first: a trench down to firm ground, wider than the wall (Foundations and Floors).
  2. Thickness: 45–60 cm for a single-storey house, 60–75 cm for two storeys. Like a dry wall, it has two faces and a core.
  3. Wet the stones before laying in hot weather, so they don't suck the water out of the mortar.
  4. Bed each stone on a full layer of mortar, push and wiggle it down until mortar squeezes out, and fill every gap in the core with mortar and small stones. Do not let stone touch stone without mortar between — except where it is pinned for level — and leave no voids.
  5. Bring up level. Every 30–60 cm of height, bring the whole wall up to a level course across its full length; this spreads the load evenly.
  6. Through-stones (or long bond stones reaching two-thirds through from alternate sides) at least one per square metre.
  7. Quoins and jambs. Build corners and the sides of doors and windows first, of your best stones, plumbed carefully. Then stretch lines between them and fill in.
  8. Pace. No more than about 1 m of height per day in lime mortar; the lower courses must stiffen. Keep fresh work damp and shaded for a week, and protect it from frost.
  9. Point the joints when the wall is done: rake out loose mortar 1–2 cm deep, wet, and press in fresh lime mortar, finishing it flush or just behind the stone face. Never point soft stone with a mortar harder than the stone.

Method 3: Ashlar

Ashlar is stone cut into accurate rectangular blocks with fine joints of 3–6 mm. It is slow and needs good tools and good stone (fine-grained sandstone or limestone are easiest), but it makes the strongest, straightest walls. It is often used only for the corners, door and window surrounds, or as a facing over a rubble core.

Dressing a block:

  1. Pitch off the big lumps with a broad, blunt pitching tool struck hard near the edge.
  2. Draft a margin. With a flat chisel, cut a narrow flat band, 2–3 cm wide, along one edge of the face. Cut a second margin on the opposite edge, checking with two straight-edges ("boning") that the two margins lie in the same plane. Then cut the other two margins.
  3. Dress the face between the margins: first with the point to knock down the bumps, then the claw chisel, then the flat chisel, until a straight-edge lies flat in every direction.
  4. Square the next face from the first using a square, and so on, until the block is a true rectangular box.

Lay ashlar on thin beds of lime mortar, with each block checked for level, plumb and line. Without iron chisels, hard stone can be shaped by pounding with harder hammerstones (Stone Tools) — slow, but the Inca built some of the finest masonry in the world this way.

Plumb, level and line

  • Plumb. Check every corner and jamb, every few courses, with a plumb line or a plumb rule: a straight board with a line down its centre and a plumb bob hanging in a hole near the bottom. When the string lies on the line, the edge is vertical.
  • Level. An A-frame level, a water level, or a plumb rule held against a long straight board at right angles (Measurement from Scratch).
  • Line. Lay every face to a tight string, raised course by course. A wall built by eye wanders.
  • Gauge rod. A rod marked with the height of each course keeps both ends of a wall rising together.

Lintels

A lintel is a beam across the top of a door or window.

Relieving archcarries the wall abovearound the lintel Stone lintelat least 20–25 cm deep,laid on its natural bed Small trianglethe only load on the lintel clear span 1–1.2 m at most Bearing15–20 cm or more each end weight of the wall
Fig. 3 A stone lintel and a relieving arch. The lintel must bear well into the wall on each side. Above a wider opening, a relieving arch carries the wall's weight around the lintel, which then only carries the small triangle of wall under the arch.
  • Use a sound, unflawed stone with no cracks or soft beds. Tap it: it must ring.
  • Keep stone lintels short: a clear span of no more than about 1–1.2 m, and at least 20–25 cm deep. Deep is what matters: a lintel twice as deep carries four times the load.
  • Each end must rest at least 15–20 cm on solid wall.
  • Lay the lintel with its natural layers horizontal.
  • For wider openings, build a relieving arch of stones or bricks in the wall above the lintel, or make the opening itself an arch (Arches, Vaults and Domes). A timber lintel (oak, see Timber Framing and Log Building) also works, but it can rot or burn.

How to tell it worked

  • Sight along the wall: its faces are straight and its top is level or follows the ground evenly.
  • No running joints: you can't trace a vertical crack line more than one course.
  • Push hard on the top of a dry wall: nothing moves. Stand on the coping: no stone rocks.
  • A plumb line held against a corner of a mortared wall hangs evenly from top to bottom.
  • After the first winter, no stones have fallen, no faces have bulged, and the mortar has not crumbled.

Note Troubleshooting. A dry wall bulges → loose hearting, too few throughs, or stones laid along the face instead of into it. Take it down to below the bulge and rebuild. Stones keep rocking → pin them from inside; choose stones with flatter beds. A wall leans or cracks from the bottom → weak or wet foundation (Foundations and Floors). Mortar crumbles → it dried too fast, froze, or had dirty or rounded sand. Rake out and repoint. Stones flake and crumble after a frost → poor, thirsty stone, or layered stone laid on edge. Replace them with tested stone laid on its bed. A lintel cracks in the middle → too long or too shallow. Prop it immediately and build a relieving arch above.

Dangers

Danger Heavy stones crush hands and feet and fall from walls. A stone the size of a bread loaf weighs 10–15 kg; a lintel can weigh half a tonne. Never put fingers under a stone you are lowering — set it down on small wooden blocks, then lever it into place. Wear stout boots. Never stand on the downhill side of a stone being levered or rolled. Build scaffolds and ramps strong enough for the stone and the people (Scaffolding and Ladders).

Danger Freshly built and old walls can collapse. A tall mortared wall is weak until its mortar hardens, and a bulging or undermined old wall can fall without warning. Prop doubtful walls, never dig beside the foot of a wall, and keep children away from walls under construction.

  • Flying chips. Chiselling and hammering throw sharp stone chips at the eyes. Protect your eyes — goggles of fine wire mesh or of glass in a leather mask, or at the very least turn your face away as you strike — and keep others back.
  • Stone dust. Cutting sandstone, granite and flint makes fine quartz dust that scars the lungs over years (silicosis). Work outside, wet the stone, and cover your nose and mouth.
  • Strain. Lift with your legs, keep the stone close, and use levers, rollers and ramps for anything you cannot lift easily.
  • Lime mortar burns skin and eyes — see Lime.

Going further

How it was first done

People were building dry stone walls before they farmed. At Göbekli Tepe in Turkey, about 11,500 years ago, hunter-gatherers raised dry stone enclosures around carved stone pillars weighing several tonnes. At Skara Brae in Orkney, around 3100 BC, a village of dry stone houses — with stone beds, shelves and hearths — still stands. Egyptian masons cut fine limestone and granite ashlar for the pyramids around 2600 BC with copper tools, abrasive sand and hammerstones of harder rock. The great curving dry stone walls of Great Zimbabwe were built between about the 1100s and 1400s AD, and Inca masons in Peru fitted many-sided granite blocks so closely, with no mortar, that a knife blade cannot enter the joints. Across Britain, Ireland and the Mediterranean, many thousands of kilometres of dry stone field walls, many centuries old, still stand.

Source: content/entries/building/stone-masonry.md