Hardened steel balls rolling between hardened tracks cut friction to a twentieth of a good plain bearing. How to forge and rough-grind balls, lap a whole batch round and equal between grooved plates, harden them, sort them by size to a few thousandths of a millimetre, and make the races, cages and rollers that carry them.

Difficulty
●●●●●
Time
A week to make a lapping machine; two to three days for a batch of a few hundred balls; a day to make and harden a pair of races
Steps from zero
21 prerequisites →

You need first

Bearings and LubricationMachine Tools

This unlocks

Gyroscopes and Inertial Guidance
The full path from nothing — 21 steps before this one
  1. Stone Tools
  2. Cordage and Rope
  3. Fire
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. The Wheel and Axle
  12. Bellows
  13. The Lathe
  14. Copper Smelting
  15. Iron (the Bloomery)
  16. Bronze
  17. Blacksmithing
  18. Steel
  19. Bearings and Lubrication
  20. The Steam Engine
  21. Machine Tools
  22. Making Ball and Roller Bearings

Do them roughly in this order. See it on the tech tree →

Why it matters

A plain bearing — a shaft turning in bronze or babbitt (Bearings and Lubrication) — works beautifully once it is running fast on a film of oil. But it drags when starting, wears whenever the oil film breaks, needs constant oiling, and wastes power when slow or lightly loaded. Rolling bearings replace sliding with rolling. A good ball bearing has a friction coefficient of about 0.001–0.003, starts as easily as it runs, needs only a little grease once in a while, and can take loads from the side and along the shaft at the same time.

That makes possible a The Bicycle that one person can pedal at 20 km/h, fast electric motors and generators, the precise spindles of Machine Tools, The Motor Vehicle and railway wheels, Gliders and Aeroplanes engines, Textile Machinery spindles turning thousands of times a minute, and turntables for Cranes and Lifting and The Windmill caps.

Be honest about the difficulty. A ball bearing only works if the balls are all the same size to within a few thousandths of a millimetre, truly round, and glass-hard, running in tracks that are just as hard and smooth. A batch of soft or unequal balls fails in hours. This is precision work, and it needs a good The Lathe, true flat plates and a micrometer (Precision and Interchangeable Parts) before you start. The good news is that the core trick — lapping a whole batch between grooved plates — is simple, and makes the balls equal almost by itself.

How it works

Why balls must be hard and equal

A ball touches its track at a tiny spot. A load of 50 kg on one 6 mm ball presses on a contact patch smaller than a pinhead, at a pressure of thousands of times atmospheric. Only fully hardened high-carbon steel (about 60 on the hardness scale — so hard a file skates off it) survives this without being dented. Soft steel flattens; the balls wear flats, rattle and jam.

If one ball is even 0.01 mm bigger than the rest, it carries nearly all the load, runs on a high spot each time round, and cracks or flakes. In a good bearing the balls of one set differ by less than 0.002–0.005 mm — about a twentieth of the thickness of a hair.

Why lapping between plates makes balls round and equal

Put a batch of rough balls in a circular groove between two plates, sprinkle in abrasive and oil, press the plates together and turn one of them. Two things happen at once:

  • Each ball tumbles. The ball touches the groove at points at slightly different distances from the centre, so it cannot roll cleanly; it slips and spins about an axis that keeps wandering. Over thousands of turns every part of its surface meets the plates. High spots — the parts farthest from the centre — touch hardest and are ground away first. The ball gets rounder.
  • Big balls are ground fastest. The biggest balls in the groove hold the top plate up and carry most of the load, so they are ground hardest until they are no bigger than the rest. If you keep mixing the balls between grooves, the whole batch is driven towards one size.

This is the same idea as making three flat plates by rubbing them on each other (Machine Tools): you do not need a perfect machine, because the errors average out.

Side section Lower plate seen from above Turned by crank or belt20–60 turns a minute Weights2–5 kg per ball upperplate turns balls lower platefixed 90° V-groovesemery and oil between plate and balls gap tray: stir feed back into a different groove
Fig. 1 The ball-lapping machine. Balls run in concentric V-grooves between a fixed lower plate and a turning upper plate, with abrasive in oil. A gap in each groove lets balls leave and be mixed back into other grooves, so the whole batch becomes round and equal.

What you need

Item Notes
High-carbon steel rod About 1% carbon (Steel). Best: 1% carbon, 1–1.5% chromium "bearing steel" (Alloy and Stainless Steels), which hardens right through even thick balls
Low-carbon steel or wrought iron For case-hardened cups and cones (Steel, carburising)
Two cast-iron lapping plates 30–40 cm across, 4–5 cm thick, faces scraped flat (The Blast Furnace and Cast Iron)
Abrasive Emery in graded sizes, coarse to flour; rouge or tripoli for polishing (Abrasives and Grinding Stones)
Oil Non-drying plant oil or mineral oil, to carry the abrasive
Swage block or ball swages Hemispherical dies for forging slugs (Blacksmithing)
Lathe with a form tool For turning races, cones and rollers
Micrometer reading 0.01 mm, and a lens Precision and Interchangeable Parts
Quench oil, an oil bath and a thermometer Hardening and tempering (The Thermometer)
Sorting rails Two hardened, ground steel bars 50–80 cm long
Sheet brass or thin steel For cages (Sheet Metal and Rolling, Zinc and Brass)

Method 1: Making steel balls

These numbers are for a batch of a few hundred balls 6 mm across. Scale them for other sizes.

1. Cut slugs

Cut short pieces of rod the same diameter as the finished ball and three-quarters as long (a 6 mm rod cut into 4.5 mm pieces). That gives about 12% more metal than the ball needs, which becomes the flash and the grinding allowance. Cut them all the same length with a stop on the saw or lathe — equal slugs make equal balls.

2. Forge them round

  1. Make a pair of ball swages: two steel blocks each with a hemispherical cup the size of the ball plus 0.3 mm, one to sit in the anvil's square hole, one with a handle (or set them in a small drop-hammer — Cranks, Cams and Linkages).
  2. Heat a dozen slugs at a time to bright orange (about 1,000 °C) in a small charcoal fire.
  3. Set a slug end-up in the lower swage, put the upper swage on it, strike firmly. Turn the slug a quarter-turn and strike again. Two or three blows make a ball with a thin ring of squeezed-out metal round its waist — the flash.
  4. Drop each into dry ash or lime to cool slowly (Lime). This leaves the steel soft enough to grind.

For a small batch, or with no swages, turn the balls on the lathe: turn a row of balls on the end of a rod with a curved form tool, leaving each joined by a thin neck, then part them off. Leave 0.3–0.4 mm extra all round for grinding.

3. Rough grinding (soft)

  1. Make the plates. In the face of the lower plate, turn 4–6 concentric V-grooves with a 90° angle, each about as deep as one third of the ball diameter. The upper plate is flat and sits on the balls. Cut a gap across all the grooves of the lower plate, a little wider than a ball, with a sloping chute so balls roll out into a tray.
  2. Mount it. Fix the lower plate level; turn the upper plate slowly (20–60 turns a minute) by a crank, treadle or belt from line shafting (Belts, Chains and Power Transmission). Press it down with weights so each ball carries 2–5 kg.
  3. Load the grooves with balls, nearly touching, and a slurry of coarse emery in oil.
  4. Run and mix. Balls slowly creep round and drop out at the gap. Every 10–15 minutes, stir the tray and feed the balls back into different grooves. Add abrasive when the slurry turns grey and stops cutting.
  5. Check every hour with the micrometer, measuring each sample ball across three directions. Stop when the flash is gone and the balls are round to about 0.02 mm, still about 0.05–0.1 mm oversize.

Rough grinding takes several hours.

4. Harden and temper

  1. Wash the balls free of abrasive.
  2. Heat them evenly in a closed iron box with a little charcoal dust (which stops the surface losing carbon) to about 800 °C: a clear cherry red, and a little hotter than the point where the steel stops sticking to a magnet. For chromium bearing steel, about 840 °C.
  3. Quench by tipping them all at once into a bucket of oil, stirring. Water is faster but cracks balls.
  4. Test a few with a file: it must skate off without biting.
  5. Temper at once in an oil bath at 150–180 °C for one to two hours (use a The Thermometer). This takes away brittleness while keeping them almost glass-hard. Do not temper to straw or blue colours as you would a tool or a spring: the balls would be too soft.

5. Lap them to size and finish

Use a second, clean pair of plates (or re-face the first). Lap exactly as before, but with fine emery, then flour emery, then rouge or tripoli in oil, mixing constantly. Measure often; take each grade down until the scratches of the previous one are gone. You are removing only the last 0.05–0.1 mm. Finish when the balls are mirror-bright with no dull spots or pits under the lens. Wash every trace of abrasive out with clean oil or paraffin.

6. Sort them

Even a good batch differs by a few thousandths of a millimetre. Sort it:

  1. Set two hardened, ground straight bars side by side, sloping gently downhill, with a gap between them that widens slowly along their length — for example from 5.98 mm at the top to 6.02 mm at the bottom.
  2. Roll the balls one by one down the gap. Each ball rides on the two bars until it reaches the place where the gap equals its diameter, and drops through into a row of boxes below.
  3. Each box is one size grade. Use balls from one box only in any one bearing.
1. Slugrod, ¾ as longas it is thick 2. Forgein swages at orangeheat; flash at waist 3. Lap softcoarse emery;0.05–0.1 mm oversize 4. Harden800 °C, oil quench;temper 150–180 °C 5. Lap and polishfine emery, then rouge;round to 0.002 mm Sorting: two hardened bars, the gap widening downhill 5.99 mm6.00 mm6.01 mm6.02 mm balls roll in here (gap exaggerated) bins: one size each
Fig. 2 From slug to sorted ball. A slug of rod is forged in ball swages, leaving a flash; lapped soft; hardened; lapped and polished. Finished balls roll down two slightly diverging bars and drop through into bins where the gap equals their size.

Method 2: Races, cages and assembly

The tracks the balls roll in — the races — must be as hard and smooth as the balls.

The cup-and-cone bearing (build this first)

The bicycle hub's bearing is the easiest to make and the most forgiving, because it can be adjusted as it wears.

  1. Turn the cup: a ring of low-carbon steel with a curved track inside, pressed into the end of the hub. Turn the cone: a short sleeve with a sloping, curved track, threaded to screw onto the axle. Shape both tracks with a form tool whose radius is about 52–55% of the ball diameter — a little larger than the ball, so the ball touches along a narrow band, not at the edges.
  2. Case-harden cup and cone: pack them in charcoal and bone-char in a sealed box and hold at bright cherry-orange for 2–4 hours (Steel, carburising), then quench in water and temper lightly at 150–180 °C. This gives a glass-hard skin about 0.5 mm deep over a tough core.
  3. Lap the tracks with a brass or cast-iron lap of the same shape, charged with fine emery in oil, the part turning in the lathe. Polish with rouge.
  4. Assemble with thick grease holding the loose balls in the cup — one ball fewer than will fit, so they do not rub together. Screw the cone in until the axle has no shake, then back it off just enough that it turns freely, and lock it with a washer and locknut.

The thrust bearing

For loads along the shaft — a turntable, a drill spindle, a crane post, a lathe tailstock screw — make two thick washers with a matching circular groove in each face, and a ring of balls between them in a flat cage. It is the easiest precision bearing of all, and a good place to test your first batch of balls.

The deep-groove radial bearing

The modern standard bearing: an inner ring with a groove round its outside, an outer ring with a groove round its inside, a ring of balls, and a cage (retainer) to space them.

  1. Turn both rings from high-carbon or bearing steel, leaving grinding allowance. Harden right through (as for balls) and temper.
  2. Grind and lap the grooves (Precision Grinding); make the groove radius 52% of the ball diameter on the inner ring, 53% on the outer.
  3. Assembly: set the inner ring against one side of the outer ring. Drop in as many balls as will fit in the crescent-shaped space (about half the number that would fill the ring). Push the inner ring to the centre, spread the balls evenly round, and fit the cage.
  4. The cage: two rings pressed from sheet brass or thin steel with half-pockets for the balls, closed round them from both sides and riveted between each pair of balls.
  5. Aim for a barely-felt radial play — on a 30–50 mm bearing, about 0.01–0.02 mm.
Cupin the hub Conescrews on; adjust it locknut loose balls in grease axle Cup and cone Deep-groove radial outer ring inner ring brasscage Thrust load alongthe shaft groovedwashers balls turntables, drill spindles, crane posts Roller roller outer ring inner ring shaft line contact: carries more load, little thrust
Fig. 3 Kinds of rolling bearing. The adjustable cup-and-cone of a bicycle hub; the deep-groove radial bearing with inner and outer rings and a cage; the thrust bearing for loads along the shaft; and the cylindrical roller bearing for heavy loads.

Method 3: Roller bearings

Rollers are easier to make than balls, because the lathe makes cylinders naturally, and they carry far more load for their size because they touch along a line instead of at a point. They cannot take much thrust.

  1. Cut rollers from high-carbon rod, each about as long as it is thick (up to one and a half times). Chamfer or round the ends slightly so the edges do not dig in.
  2. Harden and temper as for balls.
  3. Grind them all to one diameter. Set a stop so each roller is ground in exactly the same way, or roll them between two flat lapping plates with fine abrasive, mixing them often, just as for balls. Sort and match them to within 0.005 mm.
  4. Run them in a hardened bore and on a hardened shaft or inner ring, held apart by a cage. For heavy slow loads — cart axles, mill shafts, crane turntables — even rollers matched to 0.05 mm, running in a cage between cast-iron tracks, are a huge improvement over grease and wood (Bearings and Lubrication).
  5. Needle rollers — thin rollers 3–10 times as long as they are thick, packed side by side with no cage — can be cut from hardened, drawn steel wire (Iron and Brass Wire). They make compact bearings for pins and rocking levers.
  6. Tapered rollers, running between cone-shaped races, take load from the side and along the shaft at once; they suit vehicle wheels. They need more exact grinding: the rollers and the races must all point to the same spot on the axis.

Using them

  • Fits. The ring that turns with the load is a light press fit on its shaft (about 0.01 mm tight); the other ring a sliding push fit in its housing, so it can creep slightly and wear evenly. Press only on the ring you are fitting — pushing an inner ring on by its outer ring dents the tracks.
  • Load. As a rough guide, the most a well-made, fully hardened radial ball bearing can carry standing still without denting its tracks is, in newtons, about 12 × number of balls × (ball diameter in mm)². Ten 6 mm balls: about 4,300 N, roughly 440 kg. A bearing that must run for thousands of hours should carry no more than about a fifth of that; for home-made bearings, plan on a tenth (about 45 kg for this example) and test.
  • Grease with lime grease or a fine non-drying oil (Lubricants and Greases). Assemble and grease in a clean, dust-free place; makers of precise bearings work in a clean room. Fill only a third of the space; too much grease churns and heats.
  • Keep dirt out with a felt washer soaked in oil (Felt), or a narrow labyrinth of grooves. One grain of sand rolled under a ball dents the track for ever.

How to tell it worked

  • Micrometer. Balls from one bin measure the same within 0.002–0.005 mm in every direction.
  • Lens. Mirror-bright, with no flats, pits or dull bands.
  • The file and drop tests. A file skates off. Dropped from 1 m onto a hardened steel anvil, a hard ball bounces back high and rings; a soft one thuds and barely bounces.
  • Crush one. Squeeze a sample ball between two hardened plates in a press or big vice. A good ball takes a large load and then shatters; a soft one flattens.
  • Spin test. Hold the inner ring and flick the outer one: it should spin smoothly and quietly for a long time and slow down gently. A rough, gritty or notchy feeling, or a rumble when you hold a stick between the housing and your ear, means dirt, dents or unequal balls.
  • Running. After an hour's work the housing should be no more than warm to the hand.

Note Troubleshooting. Balls stay out of round → not enough mixing, too little load on the plates, or grooves worn out of shape; mix every few minutes, add weight, re-cut the grooves. Some balls much smaller than others → they spent longer in the outer grooves (which travel faster); mix between grooves more often. Balls crack in quenching → water quench, too hot, or sharp flash left on; use oil and grind off the flash first. Balls soft after quenching → not hot enough, too little carbon, or surface carbon burnt out; use a box with charcoal dust, check the steel. Bearing notchy after a few hours → tracks dented by overload or dirt, or races not hard; harden properly, keep dirt out, do not hammer bearings on. Bearing runs hot → too tight (no play), too much grease, or the shaft and housing out of line. Surface flakes after long service → that is the normal end of a rolling bearing's life (fatigue); if it comes early, it is overloaded or the steel has slag streaks.

Dangers

Danger Quench oil fires. Hot steel tipped into a small pot of oil can set it alight. Use a large metal bucket with a lid at hand, at least 10 litres of oil, plunge quickly and fully, and keep water away from hot oil — it explodes into steam and spatters burning oil.

  • Hardened steel shatters. Crushing tests and pressing hardened rings send sharp splinters flying. Wear eye protection and work behind a guard.
  • Grinding dust. Sandstone and sand slurries contain quartz; dry quartz dust scars the lungs (silicosis). Keep abrasives wet with oil, and never grind dry indoors.
  • Pinch points. The turning upper plate of a lapping machine, belts and line shafts catch fingers and clothing. Guard them.
  • Forging. Hot slugs fly out of swages. Wear leather and eye protection (Blacksmithing).

What this unlocks

Rolling bearings make the The Bicycle light and easy, let motors, generators and turbines spin fast without constant oiling, and give Machine Tools precise, play-free spindles. They are a step towards The Motor Vehicle and Gliders and Aeroplanes engines, railway axle boxes, and the fast spindles of Textile Machinery. Ball-making is also a training ground for mass precision: thousands of identical parts made to gauge (Precision and Interchangeable Parts).

How it was first done

Rolling elements are old: the Roman Nemi ships (about AD 40) carried turntables on bronze balls and wooden rollers, and Leonardo da Vinci sketched caged ball bearings around 1500. Philip Vaughan of Carmarthen, Wales, patented a ball bearing for carriage axles in 1794. In 1869 the Paris bicycle mechanic Jules Suriray patented a ball bearing for bicycle hubs, and a bicycle fitted with his bearings won the first long-distance road race, Paris–Rouen, that November.

The bicycle boom created the demand for millions of accurate balls. In 1883 Friedrich Fischer of Schweinfurt, Germany, built a machine that ground steel balls between plates to equal size — the start of the bearing industry in that town. Henry Timken of St. Louis patented the tapered roller bearing in 1898, and Richard Stribeck in Germany published careful tests of ball loads and steels around 1900–1901, which led to the 1% carbon, 1.5% chromium bearing steel still used today. In 1907 the Swedish engineer Sven Wingquist invented the self-aligning ball bearing and founded the SKF company to make it.