◆ Rebuild

Part 5 · Cloth and Clothing

Rayon and Nylon

Man-made fibres — first by dissolving cellulose from cotton or wood and squeezing it through tiny holes into an acid bath (rayon), then by building fibre molecules from scratch (nylon, polyester). How they work, the one route you can realistically try at small scale, and what a full industry needs.

Difficulty
●●●●●
Time
A few grams of cuprammonium rayon in a weekend once you have the chemicals; viscose and nylon need a chemical works
Steps from zero
14 prerequisites →

You need first

Early PlasticsSulfuric Acid

This unlocks

—
The full path from nothing — 14 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Sulfur
  4. Pottery
  5. The Kiln
  6. Lime
  7. Lye and Potash
  8. Fermentation
  9. Glass
  10. Saltpeter
  11. Distillation
  12. Sulfuric Acid
  13. Nitric Acid
  14. Early Plastics
  15. Rayon and Nylon

Do them roughly in this order. See it on the tech tree →

Why it matters

Natural fibres (Flax, Hemp and Linen, Wool, Cotton, Silk) are good, but each has limits. Silk is fine, strong and glossy, but slow and costly to raise. Cotton needs a warm climate. Short fibres must be spun; their strength depends on the twist.

A man-made fibre is a continuous filament of any thickness you choose, as long as you like, made in a factory from cheap raw materials. The first ones — rayon, "artificial silk" — gave silky cloth from cotton waste and wood. Rayon also made tyre cord, cellophane film, sausage skins and sponges. The fully synthetic fibres that followed, nylon and polyester, are stronger than any natural fibre for their weight: parachutes, ropes, fishing nets, stockings, tents, sails, conveyor belts, seat belts.

Be clear about the cost. Rayon needs strong alkali, strong acid and, for the main industrial process, a dangerous solvent. Nylon and polyester need a petrochemical industry (Petroleum and Refining, Coal and Coke). In a rebuilding world they come late, after the chemistry in Sulfuric Acid, Soda Ash and Baking Soda, Ammonia and Early Plastics is working. Until then, natural fibres are better value. This chapter explains the principles so they are not lost, and gives the one small-scale route that is genuinely achievable.

How it works

Every fibre — cotton, silk or nylon — is made of long chain molecules (polymers: molecules built of thousands of small units joined end to end, like beads on a string). A fibre is strong when those chains are long and lie parallel along the fibre, packed tightly together.

Spinning dopecotton dissolved in copper–ammonia;thick, deep blue 1–2 m head Glass nozzledrawn in a flame, 0.3–0.5 mm Blue stream turns whitecopper and ammonia leave; cellulose sets Acid bathabout 10% sulfuric acid Reel wind slowly; a gentlepull stretches the thread
Fig. 1 Wet spinning at small scale. A thick solution of cellulose runs down from a raised bottle and out of a fine glass nozzle into an acid bath, where it sets into a solid thread that is drawn out and wound on a reel. A factory does the same through spinnerets with hundreds of holes.

To make a fibre you need three steps:

  1. Make the chains into a liquid — either dissolve them (rayon) or melt them (nylon, polyester).
  2. Squeeze the liquid through a spinneret: a plate with one or many fine holes, each 0.05–0.5 mm across. Each hole makes one filament. (Silkworms and spiders do exactly this.)
  3. Make it solid at once and stretch it. For rayon, the jet enters a bath of acid that turns the dissolved cellulose back into solid cellulose (wet spinning). For nylon, the jet simply cools in air (melt spinning). Then the filament is drawn — stretched to several times its length — which lines up the chains and multiplies its strength.

Rayon is called a regenerated fibre: the chains are cellulose from plants, the same molecule as cotton and wood, dissolved and re-formed into a long filament. Nylon is a synthetic fibre: its chains are built from small molecules by a chemical reaction (polymerisation).

What you need (cuprammonium rayon, small scale)

Item Amount Notes
Copper sulfate 10 g of blue crystals From copper or malachite and sulfuric acid; see below
Lye Enough to precipitate the copper — about 25 mL of strong caustic lye Caustic soda or caustic potash (Lye and Potash, Soda Ash and Baking Soda)
Strong ammonia solution 50–100 mL, as strong as you can make it Ammonia
Cotton 1–2 g, clean, white, de-waxed Boiled in lye-water and rinsed (Cotton)
Dilute sulfuric acid 1–2 litres, about 10% Sulfuric Acid — always add acid to water
Glassware A stoppered bottle, a funnel, cloth filters, a glass tube drawn to a fine nozzle Glass, Laboratory Glassware
Reel A wooden spool or frame to wind the thread

Where to find it

  • Cellulose: the purest easy source is cotton — new cotton wool or the short fuzz (linters) left on cotton seeds after ginning. Old white cotton or linen rags also work. Industry uses wood pulp from spruce, pine or beech, cooked and bleached as for fine Paper.
  • Copper: native copper or malachite — the bright green copper ore (Finding and Identifying Ores, Copper Smelting). Malachite dropped into dilute sulfuric acid fizzes and gives a clear blue solution of copper sulfate; boil it down and blue crystals grow as it cools.
  • Ammonia: from stale urine or from heating bone and horn, distilled with slaked lime and absorbed in cold water (Ammonia). It must be strong — its smell should make your eyes water at arm's length.
  • Caustic soda: soda ash (Soda Ash and Baking Soda) boiled with slaked lime from limestone (Lime), exactly as caustic potash is made from potash in Lye and Potash.
  • Sulfur and charcoal — for carbon disulfide in the viscose process (outline only, below): Sulfur, Charcoal.

Method 1: Cuprammonium rayon (achievable)

Cellulose will not dissolve in water, acid, alcohol or oil. But it does dissolve in a deep-blue solution of copper and ammonia called Schweizer's reagent. Squirted into acid, the copper and ammonia are pulled away and the cellulose comes back out as a solid thread. This is how the fine "Bemberg" rayon was made for most of the 20th century, and it needs no poisonous solvent.

  1. Make copper hydroxide. Dissolve 10 g of copper sulfate crystals in 100 mL of cold water. Add lye a little at a time, stirring, until no more pale blue jelly forms when a drop is added. Keep it cold — if it is warmed, the blue turns black (copper oxide) and is useless.
  2. Wash it. Pour the jelly onto a fine cloth filter and rinse it with cold water 4–5 times, to wash out the salt and leftover lye. Squeeze gently. Keep it damp.
  3. Make the reagent. Put the damp blue paste into a bottle with 50–100 mL of the strongest ammonia solution you have. Stopper and shake. It dissolves to a deep royal-blue liquid. If some stays undissolved, let it settle and pour off the clear blue.
  4. Dissolve the cotton. Add the cotton in small tufts, a pinch at a time, shaking after each and keeping the bottle stoppered. Over several hours (or overnight) the cotton vanishes and the liquid becomes thick and syrupy. Add cotton until it is like runny honey. This syrup is the spinning dope. Use it within a day or two; it slowly loses its strength.
  5. Make a spinneret. Heat the middle of a glass tube in a hot flame, and when it softens pull the ends apart to draw a fine neck. Cut the neck where its hole is about 0.3–0.5 mm. Smooth the tip briefly in the flame.
  6. Spin. Fill a shallow dish with dilute sulfuric acid (about 10%). Fix the nozzle under the surface. Push the dope through steadily — with a piston in a glass tube, or from a bottle held 1–2 m higher, connected by a tube (a gravity head). As the blue stream enters the acid it turns pale and then colourless: copper and ammonia are leaving it, and cellulose is setting.
  7. Draw and wind. Pick up the end of the thread with a glass rod, lead it out of the bath, and wind it slowly onto the reel. Pulling it gently while it is still soft stretches it, makes it thinner and stronger. (The industrial process stretched the filaments in a funnel of flowing water before the acid.)
  8. Wash the reel of thread in clean water until the water no longer tastes or tests acid, and dry it in the shade.

You will get a few grams of glossy, fine filament — enough to prove the process, test it, and learn. Cellophane — clear film — is made the same way: spread the dope thinly on a glass plate and slide it into the acid bath.

Method 2: Viscose rayon (outline: an industrial process)

Viscose is cheaper than cuprammonium in bulk and became the main rayon of the world. It needs a dangerous chemical, carbon disulfide, and is not a home or village process. In outline:

1. Cellulosewood pulp orcotton linters 2. Steepin 18% caustic soda,press and shred 3. Age1–3 days at 25 °C;chains shorten 4. Xanthatechurn with carbondisulfide: orange crumb 5. Dissolvein 6–7% caustic soda:viscose syrup 6. Ripena few days; filter;remove bubbles 7. Spinspinneret into warmacid + salt bath 8. Finishstretch, wash, bleach,dry: rayon Cellophanethrough a slit, not holes red triangles: steps that give offcarbon disulfide or hydrogen sulfide —closed, ventilated plant only
Fig. 2 The viscose process. Cellulose is soaked in caustic soda, aged, treated with carbon disulfide to make an orange crumb, dissolved back in weak caustic soda to make the viscose syrup, ripened, and spun into an acid bath. Pushed through a narrow slit instead of holes, the same syrup makes cellophane.
  1. Steep sheets of purified wood pulp or cotton linters in caustic soda solution (about 18%) for 1–4 hours. Press out the excess and shred the swollen alkali cellulose into crumbs.
  2. Age the crumbs for 1–3 days at about 25 °C. Air slowly shortens the cellulose chains so the final syrup is not too thick.
  3. Xanthate: tumble the crumbs in a closed churn with carbon disulfide (roughly a third of the weight of the cellulose) for 1–3 hours. They turn into orange cellulose xanthate.
  4. Dissolve the crumb in weak caustic soda (about 6–7%) to make viscose — a thick, honey-coloured syrup of about 7–9% cellulose. Hence the name: it is viscous.
  5. Ripen it for a few days, filter it, and let the air bubbles out.
  6. Spin: pump it through spinnerets with many holes 0.05–0.1 mm across (made of gold–platinum alloy, which resists the acid) into a warm bath (40–55 °C) of dilute sulfuric acid with sodium sulfate and a little zinc sulfate. The acid regenerates the cellulose; the salts slow it down so the filaments set evenly. The bath gives off hydrogen sulfide and carbon disulfide fumes.
  7. Stretch, wash, desulfurise, bleach and dry. Continuous filament is wound up; or a thick bundle (tow) of thousands of filaments is cut into short staple to be spun like cotton (Spinning and Weaving Cloth, Textile Machinery).

Carbon disulfide is made by passing sulfur vapour over red-hot charcoal (about 800–1,000 °C) in a sealed retort and condensing the vapour under water. It is mentioned here so the process is understood. Do not attempt it without a proper chemical works and the training to run one.

Method 3: Nylon and polyester (outline)

Fully synthetic fibres are made from small molecules that react to form long chains.

  • Nylon 6,6 is made by reacting two chemicals, adipic acid and hexamethylenediamine, in equal numbers of molecules. Heated together, they join end to end into long chains and give off water. The molten nylon is cast, chopped, remelted at about 280 °C, and pushed through a spinneret into cool air. Both raw chemicals come from benzene (from coal tar, Coal and Coke, or from Petroleum and Refining) through several steps, including oxidation with nitric acid (Nitric Acid) and reaction with hydrogen (Hydrogen, Oxygen and Gases) under pressure with catalysts.
  • Polyester (PET) is made from terephthalic acid and ethylene glycol — both from petroleum — in the same way, and melt-spun at a similar temperature.
  • Cold drawing is what makes them strong. A freshly spun nylon filament is weak and stretchy. Pulled to 3–5 times its length at room temperature, it suddenly narrows (it "necks") as the chains line up, and becomes far stronger.
COLD DRAWING A FRESHLY SPUN FILAMENT As spun The neck Drawn 3–5 times chains tangled: weak,stretches like soft wax chains side by side and packed:thin, glossy, many times stronger The neck travels along the filament as you keep pulling.
Fig. 3 Cold drawing. In the freshly spun filament the long molecules lie in a tangle. Stretching it three to five times pulls them parallel, and the fibre becomes thinner and many times stronger.

You can see cold drawing for yourself with any thin strip of soft thermoplastic — a filament you have melt-spun, or, if you have salvaged one, a strip cut from an old plastic bag: pull it slowly and steadily and watch a narrow "neck" travel along it as the strip turns thinner, clearer and stronger.

How to tell it worked

  • The burn test tells fibres apart. Hold a few threads in tongs over a candle (Lamps and Candles):
Fibre In the flame Smell What is left
Rayon, cotton, linen Burns quickly with a yellow flame, keeps burning Burning paper Soft grey ash
Wool, silk Burns slowly, curls away, often goes out Burning hair Crushable black bead
Nylon Melts and shrinks away, drips Faint celery-like Hard, round, grey-brown bead
Polyester Melts, shrinks, black sooty smoke Faintly sweet Hard black bead
  • Wet strength. Rayon loses about half its strength when wet. Pull a dry thread and a wet one: the wet one should break much more easily. (Nylon hardly changes.)
  • Lustre. Good rayon filament is glossy, like silk. Dull, chalky thread means the bath was too strong or the filament set too fast.
  • Even thickness along the thread, seen against light.

Note Troubleshooting (cuprammonium). Copper paste turns black → it got warm. Make it again with cold water and keep it cold. Cotton won't dissolve → the ammonia is too weak, or the cotton still has wax on it. Use stronger ammonia and boil the cotton in lye-water first. Thread breaks as soon as it forms → the dope is too thin, or you are pulling too fast. Dissolve more cotton; wind more slowly. Blobs instead of a thread → the nozzle is too wide or the dope is pushed too fast. Draw a finer nozzle and push gently. Thread stays blue → it has not been in the acid long enough. Use a longer path through the bath, or a stronger acid.

Dangers

Danger Carbon disulfide is poisonous and catches fire extremely easily. Its vapour ignites on its own at only about 90–100 °C — the heat of a steam pipe or a hot plate is enough, no flame needed — and it is heavier than air, so it pools and flows along floors. Breathed over weeks and months it damages the nerves, brain and heart; early viscose workers suffered madness, paralysis and heart disease. It is a factory chemical only: closed equipment, forced ventilation, and no source of heat or spark anywhere near.

Danger Strong ammonia, lye and sulfuric acid all destroy eyes and skin. Wear eye protection (glass goggles or at least a face shield of clear glass or horn), work outdoors or with strong airflow for ammonia, and keep plenty of clean water at hand to flood any splash for 15 minutes. Always pour acid into water, never water into acid. See Lye and Potash and Sulfuric Acid.

  • Hydrogen sulfide (rotten-egg gas) comes off viscose spinning baths. It kills in high doses, and at those doses it deadens your sense of smell first, so you stop noticing it.
  • Copper salts are poisonous to drink and to fish. Do not pour spent copper solutions into streams; neutralise and dry them, and recover the copper (Copper Smelting).
  • Old history: the very first artificial silk (Chardonnet's, 1884) was spun from nitrocellulose, a close relative of guncotton, and caught fire disastrously. It was abandoned for good reason; do not attempt it.
  • Melted nylon and polyester stick to skin and cause deep burns. Clothing of these fibres melts onto the skin in a fire; wear wool or cotton at forge, kiln and furnace.

What this unlocks

How it was first done

In 1857 the Swiss chemist Matthias Eduard Schweizer found that copper and ammonia dissolve cellulose. In 1884 the French Count Hilaire de Chardonnet patented "artificial silk" made from nitrocellulose, and showed it at the Paris Exposition of 1889; it was dangerously flammable. Cuprammonium fibre was made commercially in Germany in the 1890s, and the German firm of J. P. Bemberg made it a success after Edmund Thiele invented stretch spinning in 1901. In 1892 the English chemists Charles Cross, Edward Bevan and Clayton Beadle patented viscose; the firm of Courtaulds began making viscose yarn at Coventry in 1905, and the name "rayon" was adopted in the United States in 1924. Cellophane was invented by the Swiss chemist Jacques Brandenberger around 1908–1912. At the American company DuPont, Wallace Carothers's group made nylon 6,6 in 1935; nylon stockings went on sale in 1940, and during the Second World War nylon replaced silk for parachutes. In Britain, John Whinfield and James Dickson invented polyester in 1941.

Source: content/entries/textiles/synthetic-fibres.md