◆ Rebuild

Part 2 · Earth and Fire

Lime

How to burn limestone or seashells into quicklime, slake it into lime putty, and use it for mortar, plaster and whitewash. Lime is the glue of masonry and a basic chemical for farming, tanning, soap and glass.

Difficulty
●●●●●
Time
2–4 days to burn a kiln-load; weeks to months for putty to mature
Steps from zero
3 prerequisites →

You need first

The Kiln

This unlocks

Calcium Carbide and AcetylenePigments, Paints and VarnishSoda Ash and Baking SodaGlassMortar and ConcretePortland Cement
The full path from nothing — 3 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Lime

Do them roughly in this order. See it on the tech tree →

Why it matters

Burn a white stone, pour water on it, and it hisses, steams, swells and falls to a fine white powder. Mix that powder with sand and water, and it slowly turns back into stone — gluing bricks and stones together. This is lime, and it has held buildings together for ten thousand years.

Lime gives you:

How it works

Limestone, chalk, marble and seashells are all mostly the same chemical: calcium carbonate — calcium joined with carbon dioxide gas. Lime-making is a loop with three stages:

LIMESTONEchalk, marble, shells · calcium carbonate QUICKLIMEcalcium oxide SLAKED LIMEputty or powdercalcium hydroxide CO₂ out CO₂ in 1 · Burn900–1,000 °Closes 44% of weight 2 · Slakeadd to water: it boils, swells, crumbles 3 · Setin mortar andplaster, overmonths, backto stone
Fig. 1 The lime cycle. Burning drives carbon dioxide out of limestone, leaving quicklime. Water turns quicklime into slaked lime. Over months, slaked lime in mortar or plaster takes carbon dioxide back from the air and becomes stone again.
  1. Burning (calcining). Heated above about 900 °C — bright cherry to orange heat — limestone gives off carbon dioxide gas and becomes quicklime (calcium oxide). The stone keeps its shape but loses 44% of its weight: 100 kg of pure limestone gives 56 kg of quicklime. It becomes light, chalky and hungry for water.
  2. Slaking. Quicklime added to water reacts violently. It gets hot enough to boil the water, hisses, swells to two or three times its volume, and falls apart into slaked lime (calcium hydroxide) — a fine white powder, or, with more water, a soft white paste called lime putty.
  3. Setting (carbonation). Slaked lime spread out in mortar, plaster or whitewash slowly absorbs carbon dioxide from the air and turns back into calcium carbonate — limestone. It hardens over weeks, and keeps hardening for years.

Because it needs air to set, ordinary lime will not harden underwater or deep inside a thick wall where air cannot reach. Adding certain fired clays or volcanic ash changes that (see "Mortar" below).

What you need

Item Amount Notes
Limestone, chalk or shells As much as you want lime, ×2 Broken to fist size (5–10 cm)
Fuel Roughly the same weight as the stone Dry split wood; Charcoal is better if you have it
A kiln 1 A pottery The Kiln for small amounts; a lime kiln (below) for large ones
Slaking pit or large pots 1–2 Lined with clay or stone, never wood that might dry out
Long-handled hoe or paddle 1 For stirring slaking lime at arm's length
Sieve or coarse basket 1
Clean sharp sand 3 times the volume of putty For mortar and plaster
Water Plenty
Eye and skin protection See Dangers. Leather gloves, long sleeves, a cloth over nose and mouth, something to shield the eyes

Where to find it

  • Limestone is common worldwide. It forms pale grey, cream or white cliffs and outcrops, often in thick layers. Limestone country has caves, sinkholes, dry valleys, springs that leave white crusts, and streams that vanish underground. Many limestones are full of fossil shells. Marble is limestone that has been crystallised by heat underground; it burns to lime too.
  • Chalk is a very soft, pure white limestone that marks your fingers. It forms rolling white downs and sea cliffs (with dark flint nodules in it — see Stone Tools).
  • Seashells, coral and the old shell heaps left by earlier people make excellent, pure lime. Wash off sand and salt first. Shells are thin and burn easily.
  • Travertine and tufa — porous, crusty rock deposited by limy springs — also work.

The acid test. Put a drop of vinegar, sour fruit juice or any acid on the stone. Limestone, chalk, marble and shells fizz (tiny bubbles of carbon dioxide). If it fizzes strongly and steadily, it will make lime. Rock that fizzes only weakly, or only when powdered, may be dolomite — it still makes a usable lime, but a weaker one. Stone that does not fizz at all is not limestone.

Limestone can be scratched with a hard stone or steel blade but not with a fingernail (chalk can). A clay-rich, darker limestone makes a lime that sets even under water (a hydraulic lime — see Portland Cement). Note it and try it.

Burning lime

Small amounts: in a pottery kiln

For your first lime, or a few kilograms for whitewash or mortar tests:

  1. Break limestone into pieces the size of a walnut to an egg (2–5 cm). Shells can go in whole.
  2. Put them in the The Kiln, on top of or among the pottery, or fill the chamber with stone alone.
  3. Fire as usual, but hold the kiln at bright cherry to orange heat (900–1,000 °C) for at least 4–6 hours. Larger pieces need longer. Shells need 1–2 hours.
  4. Let it cool, and test it (see "How to tell it worked").

Large amounts: a lime kiln

For building, you will want tonnes of lime. A traditional flare kiln (or intermittent kiln) is a tall, thick-walled pot built into a hillside, with a fire burning under an arch of the limestone itself.

FLARE LIME KILN load from the top Stone wallsset in clay, 40–60 cmclay-lined inside Archof the largest pieces Eyestoke here; drawlime out after Fireboxfed 2–4 days and nights Chargelimestone in fist-sized pieces;glows orange to the top when done 2–2.5 mtall Earth bankholds the heat in
Fig. 2 A simple flare lime kiln built into a bank, in cross-section. The bottom courses of limestone are built into an arch over the firebox. Smaller stones are piled above. The fire is fed for two to four days until the whole charge glows orange.
  1. Build the shaft. Choose a bank or slope so you can load from the top and stoke from the bottom. Build a round shaft 1.2–1.5 m wide inside and 2–2.5 m tall, with walls of stone set in clay, 40–60 cm thick, backed by the earth of the bank. At the bottom, on the downhill side, leave an opening (the eye) about 40 cm wide and 50 cm high for stoking and drawing out lime. Line the inside with clay.
  2. Build the arch. On the floor, build an arch of the largest limestone pieces — roughly 50 cm high — spanning the shaft, with gaps between the stones for flame to pass. The space under the arch is the firebox, reached through the eye.
  3. Load the charge. On top of the arch, pile limestone broken to fist size (5–10 cm), larger pieces low and smaller ones higher, loosely enough for flame to rise through. Fill to just below the top. A shaft this size holds about 3–4 tonnes of stone.
  4. Light it gently. Start a small fire in the firebox and keep it low for the first 6–12 hours, to dry the stone and kiln. Wet limestone can burst.
  5. Fire it hard, day and night. Feed the firebox steadily with dry split wood. Flames will rise out of the top of the charge. Keep it going 2–4 days. Have a team: someone must stoke every 15–30 minutes, round the clock.
  6. Judge when it is done. The charge sinks by 10–20% as the stone shrinks. Look into the top (from the side, with care): the stones should be glowing orange right up to the top. Poke a long rod down through the charge; burnt lime crumbles and the rod goes down easily. Draw out a test piece through the eye and test it.
  7. Close and cool. Stop firing, close the eye with stones and clay, cover the top, and let the kiln cool for 1–2 days. Then draw the lime out through the eye, starting from the bottom.

Tip A continuous kiln. If you have Charcoal (or coal), fill the shaft with alternating layers of fuel and stone — about one part fuel to three or four parts stone by volume — light it at the bottom, and draw burnt lime out from the bottom every day while adding new layers on top. This saves fuel, but needs charcoal; wood flames do not work well buried in the charge.

How to tell it worked

  • Weight. A well-burnt lump feels about half as heavy as the same lump of raw limestone. This is the quickest test.
  • Look and feel. Surfaces are dull, chalky and dusty; edges crumble. A broken lump is white or pale all the way through.
  • Water test. Put a lump in a dish and sprinkle water on it. Good quicklime soaks it up, then within seconds to a few minutes it hisses, steams, cracks and crumbles into powder, getting very hot. This is the definitive test.
  • No fizz. A pinch of the slaked powder dropped in vinegar fizzes little or not at all.

Note Troubleshooting. Lumps with hard, grey, unchanged cores that won't slake → underburnt; the heat or time was not enough. Break smaller or burn longer. Pick out the cores and reburn them. Slakes very slowly, glassy-looking lumps → overburnt (rare in wood kilns), or very impure stone. Keep these wet longer; they will slake eventually. Lime pops and blisters in plaster weeks later → small unslaked bits; sieve the putty and let it mature longer before use.

Slaking

Quicklime must be slaked before use. There are two ways.

Lime putty (the best for mortar, plaster and whitewash)

  1. Prepare the pit. Use a clay-lined pit, a stone trough, or large fired pots. Fill about one-third with water.
  2. Add lime to water — never water to lime. Wearing eye protection and gloves, add quicklime lumps gradually, about 1 part lime to 3 parts water by volume. Stand back. It will start to bubble, hiss and boil within minutes.
  3. Stir and feed water. Stir with a long-handled hoe. Add more water whenever it gets thick, so it never dries out or "burns" (a dry, overheating lump turns gritty and weak). Keep stirring until it stops boiling and is a smooth, creamy paste. A batch takes 20–60 minutes.
  4. Sieve. Pour it through a coarse sieve or basket into the storage pit to remove grit and unslaked lumps.
  5. Mature it. Let it settle. Keep a layer of water 2–5 cm deep on top and cover it, so air cannot reach it. Leave it at least two weeks; three months is much better. It becomes smoother, stickier and more workable. Stored this way, under water, putty keeps for years — the Romans liked it three years old.

Dry hydrated lime (powder)

Spread quicklime lumps in a layer, sprinkle them with about a third of their weight in water (a little more to allow for steam), and cover them with a layer of sand or earth to hold in the heat. Within a day they fall into a fine dry powder. This is easier to carry and store (in dry, closed pots), but makes weaker, less smooth mortar than putty.

Using lime

Mortar

  • Basic lime mortar: 1 part lime putty to 3 parts sand by volume. Use sharp (angular), clean sand: river sand or crushed stone, washed free of clay, earth and salt. Round beach sand works poorly and must be washed of salt.
  • Mix it hard. Beat and chop the putty and sand together with a hoe or by treading for 10–20 minutes, without adding much water. It looks too dry at first, then suddenly becomes buttery. Good mortar sticks to an upside-down trowel.
  • Keep it damp, slow, and frost-free. Lime mortar stiffens in days and hardens over months. For the first week, keep fresh work damp by misting it and shading it from sun and wind. Never build in frost.
  • Faster, stronger, and waterproof: add a pozzolan — a material that reacts with lime to form hard compounds even without air. Finely crushed fired brick or pottery (see Bricks) or volcanic ash both work. Try 1 lime : 1 pozzolan : 2 sand. The Romans built harbours and baths with lime and volcanic ash this way. See Mortar and Concrete.

Plaster

  1. First coat ("scratch coat"): 1 putty : 2½–3 coarse sand, with a good handful of animal hair or chopped straw mixed into each bucket to hold it together. Wet the wall, press it on about 10 mm thick, and scratch it with a stick to give the next coat grip. Let it firm up for 2–7 days, keeping it damp.
  2. Second coat: the same mix without scratching, 8–10 mm, smoothed flat.
  3. Finish coat: 1 putty : 1 fine sand, 2–3 mm, polished smooth with a wooden float or flat stone as it stiffens.

Whitewash (limewash)

Thin lime putty with water to the thickness of skimmed milk — about 1 part putty to 3–5 parts water. Stir in a handful of salt or a little animal fat per bucket to help it last. Brush 3–5 thin coats onto a damp wall, letting each dry first. It goes on almost transparent and turns brilliant white as it dries. It kills insects and germs, so it is excellent for food stores, barns, kitchens, sickrooms and latrines.

Other uses

  • Soil. Sour (acid) soils grow better crops after a sprinkling of crushed limestone or slaked lime. See Compost and Manure.
  • Hides. Soaking hides in lime water for one to two weeks loosens the hair so it scrapes off easily. See Hides and Leather.
  • Stronger lye. Boiling wood-ash lye with slaked lime turns it into a much stronger caustic. See Lye and Potash and Soap.
  • Glass. Lime makes glass hard and stops it dissolving in water. See Glass.
  • Maize. Cooking maize in water with a little lime (about 1% by weight) frees its niacin and prevents pellagra, a deadly deficiency disease. See Grain, Flour and Bread.
  • Latrines. A scoop of lime over latrine waste reduces smell and flies. See Sanitation and Germs.

Dangers

Danger Quicklime and wet lime burn eyes and skin. Lime is a strong alkali. A speck in the eye can cause permanent blindness. Shield your eyes when breaking, slaking or mixing lime, and never lean over a slaking pit. If lime gets in an eye, flush it immediately with clean water for at least 20 minutes — hold the lids open, keep pouring, and do not rub. Then keep rinsing. Speed matters more than anything else.

Danger Quicklime plus water makes intense heat. Slaking lime boils and spits; damp quicklime stored in a pile can get hot enough to set wood, straw or cloth on fire. Ships carrying quicklime have burned when water leaked in. Store quicklime dry, in closed pots or under cover on stone, away from anything that burns.

  • Skin. Wet lime and mortar slowly burn skin — it feels slippery, then cracks and bleeds, often hours later. Wear gloves or wrap your hands; wash off splashes with plenty of water. Keep rinsing with plain water for at least 15 minutes; do not try to neutralise it with vinegar or juice. Lime in the eye is an emergency: flush with clean water for 20 minutes or more, holding the lids open.
  • Dust. Do not breathe quicklime or lime powder. Work upwind with a damp cloth over your nose and mouth.
  • Kiln gas. A burning lime kiln gives off large amounts of carbon dioxide, which is heavier than air and pools in hollows and around the kiln's base, as well as carbon monoxide. People have died from sleeping beside lime kilns for warmth. Never sleep near a burning kiln, and never climb down into a cooling kiln or pit.
  • Burns and falls. The top of a lime kiln is a pit of glowing stone. Never walk on the charge.

What this unlocks

Lime turns Bricks and stone into buildings, bridges and cisterns (see Mortar and Concrete and Roads and Bridges). Mixed with clay and burned harder, it leads to Portland Cement. It is a key ingredient of Glass and Soda Ash and Baking Soda, and helps make Hides and Leather, Soap and Sugar.

How it was first done

In the Near East, lime is older than pottery. People there were burning limestone into plaster about 12,000 years ago, and by 9,000 years ago villages there laid polished lime-plaster floors and made large plaster statues, such as those found at 'Ain Ghazal in Jordan. Egyptian builders mostly used gypsum, a cousin of lime that needs less heat (see Gypsum and Plaster of Paris). The Greeks and especially the Romans made lime mortar into a science: the Roman architect Vitruvius, writing in the first century BC, gave mixes of lime and sand, and Roman builders mixed lime with volcanic ash to make concrete that set underwater — the Pantheon's concrete dome in Rome, nearly 2,000 years old, is still standing. Until the 19th century, almost every brick and stone building in the world was held together with lime.

Source: content/entries/earth/lime.md