◆ Rebuild

Part 3 · Metals

Anvils, Trip Hammers and Power Hammers

How to make a proper steel-faced anvil, by forge-welding or casting, and then how to let water, belts and steam swing the hammer for you. Covers water-driven trip and helve hammers, mechanical and steam power hammers, and the drop hammer with closed dies that forges spanners and crankshafts by the thousand.

Difficulty
●●●●●
Time
A week to forge-weld a block anvil; a season to pattern and cast a steel-faced anvil; one to three months to build a mechanical power hammer; a drop-forging shop is the work of a small factory
Steps from zero
19 prerequisites →

You need first

BlacksmithingThe Blast Furnace and Cast IronThe Waterwheel

This unlocks

Forge Shops and Heat Treatment
The full path from nothing — 19 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. The Kiln
  10. Hides and Leather
  11. Bricks
  12. The Wheel and Axle
  13. Firebrick and Refractories
  14. Bellows
  15. Gears
  16. Iron (the Bloomery)
  17. The Waterwheel
  18. Blacksmithing
  19. The Blast Furnace and Cast Iron
  20. Anvils, Trip Hammers and Power Hammers

Do them roughly in this order. See it on the tech tree →

Why it matters

The stone anvil of Blacksmithing works, but it chips, it has no edge you can trust, no horn for bending and no holes for tools. A real anvil — a block of iron with a hard steel face — is the smith's most valuable possession. A good one lasts two hundred years and passes through ten generations of smiths.

The second limit is the arm. A 30 kg bloom, an anchor shank or a locomotive axle needs blows no person can give. Letting a The Waterwheel, then a belt, then steam lift the hammer multiplied the size of work a forge could do by a hundred. The last step, the drop hammer with closed dies, squeezes hot steel into a shaped cavity and turns out identical spanners, connecting rods and crankshafts one every few seconds. That is the forged half of Precision and Interchangeable Parts, of the The Motor Vehicle and of the Railways.

How it works

Mass under the blow. When a hammer hits work lying on an anvil, the anvil tries to move away. If it is heavy, it barely moves, and nearly all the energy goes into squashing the hot metal. If it is light, it jumps, and the blow is wasted. The rule smiths have used for centuries:

Hammer Anvil should weigh at least
Hand hammer, 1 kg 50 times as much: 50 kg, better 100 kg
Sledge, 4–5 kg 25 times: 100–150 kg
Power hammer ram or helve head 10–15 times the moving weight
Steam or drop hammer tup 10–20 times the tup

The blow is energy: weight (kg) × drop (m) × 9.8 joules. A hand hammer swung hard gives 50–100 J; a 100 kg helve head dropping 40 cm about 400 J; a 1-tonne steam hammer falling 1 m about 10,000 J.

A hard face, a soft body. The face must be hardened steel so it does not dent, and so a hammer rebounds from it instead of sinking in; the rebound lifts the hammer for the next blow and saves the smith's arm. But a whole anvil of hardened steel would shatter. So anvils are built with a tough body of wrought iron, cast iron or soft steel, and a hard skin of steel on top.

What you need

Item Use See
Wrought iron blooms or bar, 100–200 kg Block or forged anvil body Iron (the Bloomery), The Blast Furnace and Cast Iron (finery)
Steel plate, 12–20 mm thick Anvil face Steel, Steel in Quantity
Cast iron or cast steel, 150–300 kg melt Cast anvils, hammer frames The Blast Furnace and Cast Iron, Metal Casting
Oak trunk or beam, 40–60 cm thick Anvil stand, helve, frames Sawmills and Lumber
Water supply 2–3 m above the forge Hardening the face Pipes, Plumbing and Aqueducts
Leaf spring Mechanical power hammer Springs
Line shaft, belt, or motor of 1–3 kW Power hammer drive Belts, Chains and Power Transmission, The Electric Motor, Gas Engines and Producer Gas
Steam at 4–7 bar Steam hammer Boilers and Pressure Vessels
Die steel blocks Hammer and forging dies Alloy and Stainless Steels
Lathe, planer, shaper Guides, dies, rams Machine Tools

The anvil

Face hardened steel plate, welded on Rounded edge for bending Heel holes for tools Step soft: cut here Horn rings, curves Body iron, tough, not hard Waist Feet Oak stump face at knuckle height Seen from above Hardy hole square, ~25 mm Pritchel hole round, 12–16 mm
Fig. 1 The London-pattern anvil and its parts. The hardened steel face is welded to a softer body. The horn bends rings; the step (table) is soft for cutting on; the hardy and pritchel holes take tools.

Parts and proportions

The shape that most smiths settled on by 1800 is the London pattern:

  • Face — the flat, hardened top. Slightly crowned is better than dished. Round one edge near the horn to about 5–6 mm for bending; the rest 1–3 mm. Dead-sharp edges chip.
  • Horn — a tapering cone for curves and rings, about a third of the total length.
  • Step (table) — a soft ledge 2–3 cm below the face. Cut on this, never on the face.
  • Heel — the overhang with the square hardy hole and round pritchel hole (The Blacksmith's Tooling).
  • Waist and feet — narrow under the face, spreading to four feet.
Weight Face width Face length (step to heel) Height Hardy hole
25 kg 7 cm 22 cm 20 cm 19 mm
50 kg 9 cm 30 cm 24 cm 22–25 mm
100 kg 11 cm 38 cm 28 cm 25 mm
150 kg 12 cm 42 cm 31 cm 25–32 mm

A 70–120 kg anvil serves a general smith; lighter for knives, heavier for a striker. Start with the older block anvil: a plain block with a flat face, set in a stump, with a separate small horn stake in a hole beside it.

Method 1: A forge-welded block anvil

  1. Slabs. Forge bloom iron into slabs 3–4 cm thick and 10 × 25 cm, enough for 40–60 kg.
  2. Weld a stack, one slab at a time, at white welding heat (Blacksmithing), with a striker or under a trip hammer. A block 12 × 25 × 20 cm weighs about 47 kg.
  3. Face. Weld on a plate of steel (0.8–1% carbon, Steel) about 15 mm thick, both faces scale-cleaned and fluxed, working from the middle outward so slag squeezes out. Hammer every part: an unwelded patch rings dull later.
  4. Hardy hole. Punch it 2–3 cm from one end while the block is hot.
  5. Harden and temper the face as in Method 2, then grind it flat (Precision Grinding) and round the edges.

Method 2: The forged London-pattern anvil

This is how English anvil makers worked into the 20th century, with a team of strikers or a heavy helve hammer.

  1. Body. Weld up a wrought-iron core block, held by a "porter" bar welded on as a handle. Weld on the four feet, then a forged horn and heel at each end. Each weld takes many heats; a 100 kg body is a week's work for a team.
  2. Holes. Punch the hardy and pritchel holes through the heel while hot.
  3. Face. Weld on a steel plate 15–20 mm thick covering face and heel but not the step.
  4. Harden. Heat the whole top to an even cherry red, about 800 °C in a large fire. Set the anvil on a firm frame under a falling column of water from a tank 2–3 m above — a pipe 5 cm across. Run water on the face for several minutes until it is fully black, while the body stays hot. This hardens only the face.
  5. Temper. Stop the water. Heat flows back up from the body into the face. Watch a patch rubbed bright with a stone: when it turns light straw (about 220 °C), cool the face again with water. Some makers left the face untempered; a straw temper makes it less likely to chip.
  6. Finish. Grind the face flat and round its edges.

Method 3: Cast anvils

Cast iron alone makes a cheap but poor anvil. The face is soft unless it is cast against an iron chill (a thick iron plate laid in the mould, see The Blast Furnace and Cast Iron), which makes a white, hard face — but a brittle one that chips and cracks under heavy blows. Use one only for light work.

Cast iron with a steel face is far better. Make a wooden pattern of the anvil 1% oversize (Metal Casting) and mould it upside down, face at the bottom. Forge a steel face plate 15–20 mm thick with dovetail ribs on its back, heat it red and lay it face-down in the mould. Pour grey iron onto it: the iron grips the ribs and partly welds to the plate. Harden the face as above. These anvils ring very little, which many smiths prefer.

Cast steel anvils, poured whole from medium-carbon steel (0.5–0.7% carbon) and the face hardened, are the best of all. They need molten steel (Steel in Quantity, The Electric Arc Furnace) and a foundry that can pour it at 1,600 °C.

The anvil stand

Set the anvil on the end of an oak or elm stump sunk 40–60 cm into the ground, or on a stout timber frame, or on a box of packed sand. The face should be at knuckle height with your arm hanging. Hold it with iron staples or bent bars driven into the stump around the feet. A chain wrapped tight around the waist, or a bed of thin leather or cork under the feet, quietens the ring.

How to tell a good anvil

  • Rebound. Drop a hardened steel ball 2–3 cm across (Making Ball and Roller Bearings) from 25 cm onto the face. On a good face it bounces back 18–23 cm (70–90%); on soft iron 5–10 cm. A dead spot means the face has come unwelded there.
  • Ring and file. Tapped all over, it rings clearly everywhere. A file skates on the face and bites on the step.
  • Flat. A straightedge shows no gap over about 1 mm. Small edge chips are normal in an old anvil; missing pieces of face are not.

Trip and helve hammers

How to build a cam-driven hammer, its helve, cams and frame is in Cranks, Cams and Linkages and Sheet Metal and Rolling. What matters for forging:

Kind Where the cam lifts Head Lift Blows a minute Best for
Belly helve Middle of the helve 150–350 kg 30–50 cm 60–100 Shingling blooms, heavy bar
Nose helve Under the head itself 1–4 tonnes 40–60 cm 60–90 The heaviest blooms and puddled balls
Tilt (tail) hammer Presses down the tail 30–150 kg 15–25 cm 120–300 Drawing bar, scythes, spades, plate

Shingling squeezes a fresh bloom or puddled ball (The Blast Furnace and Cast Iron) into a solid lump under slow, heavy blows; a faster hammer then draws it into bar. A springy oak or ash spring beam above a tilt hammer's helve throws the head back down, faster and harder. Fit head and anvil with removable steel dies, 5–8 cm thick, wedged into dovetail slots, so worn faces can be replaced and swages or fullers swapped in. The smith works the piece with long tongs and sets the speed with the water gate.

Mechanical power hammers

Crank Connecting rod Leaf spring Toggle links Ram slides in guides Top and bottom dies Hot work Anvil (sow block) 10–15 × the ram Flywheel pulley same shaft as crank Slack belt from line shaft or motor Idler pulley pressed up: belt grips Cast-iron frame or heavy steel plate Treadle Concrete foundation
Fig. 2 A mechanical spring power hammer. A belt drives the flywheel when the treadle tightens the idler pulley. The crank pulls the leaf spring up and down, and the spring whips the ram onto the work.

A belt-driven power hammer brings the trip hammer into any workshop with a line shaft or motor, and lets one smith vary each blow from a tap to a full hit with his foot. The classic is the spring hammer.

How it works

A crank moves a leaf spring up and down; the ram, sliding in guides, hangs from the spring by links. At slow speed the ram just follows and taps. Faster, its weight lags, the spring bends and whips it down far harder than gravity alone. The drive belt is slack; a treadle presses an idler pulley against it — light pressure for soft blows, full pressure for hard ones. Let go and a brake stops the ram up.

Proportions

Ram Anvil (sow block plus base) Blows a minute Motor Largest square bar
11 kg (25 lb) 200–250 kg 250–300 0.75–1.1 kW 4 cm
23 kg (50 lb) 400–500 kg 200–250 1.5–2.2 kW 6 cm
45 kg (100 lb) 800–1,000 kg 160–200 3–4 kW 8 cm

Building a spring hammer (23 kg ram)

  1. Foundation. A concrete block 1 × 1 m and 80 cm deep with bolts cast in (Mortar and Concrete), separated from the shop floor by a 2 cm sand-filled gap so the blows go into the ground, not the building.
  2. Anvil and frame. Best is one grey-iron casting, a column 1.6–1.8 m high with the anvil base at its foot, about 450 kg (The Blast Furnace and Cast Iron). Or a solid steel base block of at least 25 × 25 × 60 cm (300 kg) with a plate column welded on (Welding).
  3. Guides and ram. Two planed guides 50–60 cm long, adjustable so the ram slides with 0.2–0.3 mm play. The ram is a steel block 10 × 10 × 30 cm with a dovetail for the top die.
  4. Spring. A cart leaf spring of 5–7 leaves, 60–80 cm long (Springs), clamped at its middle to a yoke on the connecting rod, its ends joined to the ram by two toggle links that straighten at the bottom of the stroke and whip it harder.
  5. Crank and drive. A shaft in two bearings (Bearings and Lubrication) at the top, with a crank of 7–10 cm throw, a 50–60 cm flywheel that is also the belt pulley, a slack flat belt, and an idler worked by a full-width treadle (Belts, Chains and Power Transmission).
  6. Dies. Flat dies 5 × 12 cm of medium-carbon or alloy steel (Alloy and Stainless Steels), hardened and tempered to blue (about 300 °C), edges radiused 3–6 mm, keyed into dovetails. Set them to meet while the ram is still 2–3 cm short of its lowest point; the spring does the rest.

Air hammers are smoother but need well-bored cylinders (Drills and Boring, Bellows to Air Compressors): a crank-driven piston pumps air into a second cylinder whose piston is the ram, and a hand valve chooses lift, hold, single blow or continuous hammering.

The steam hammer

When forgings grew to ship's paddle shafts and cannon-sized rolls, no cam or spring could lift the weight. The steam hammer puts a vertical steam cylinder on a tall frame directly over the anvil. The piston rod carries the tup (the falling weight with the top die).

In a single-acting hammer steam lifts the tup and it falls by its own weight; a double-acting one also drives it down, harder and faster. A hand lever works the valve, and a skilled driver can make a 5-tonne tup just kiss the work, then strike full blows. Tups of 250 kg to 5 tonnes cover most forges (the giants of the late 1800s reached 50 and even 125 tonnes). The one-piece anvil block weighs 10–20 times the tup, rests on oak timbers in a deep pit, and stands apart from the frame's foundation. Steam at 4–7 bar comes from a boiler, with a drain cock to clear water from the cylinder before starting. The very largest forgings later went to slow hydraulic presses (Hydraulic Presses and Rams), which squeeze right through a block instead of hammering its surface.

Drop hammers and closed-die forging

Rolls grip boards, lift Hardwood boards Tup 100–1,000 kg Top die Hot bar Bottom die Anvil block 20 × the tup falls 1–2 m Top die Bottom die Gutter holds spare metal Draft 5–10° slope Impression filled with hot steel Flash land gap 1.5–3 mm With flash trim Trimmed forging
Fig. 3 Closed-die drop forging. The board drop hammer lifts the tup by rolls gripping the boards and lets it fall. The hot bar is struck in the dies' impressions; extra metal squeezes into the flash gutter and is trimmed off afterwards.

Every hammer above is open-die: the smith shapes the work by moving it between flat or simple dies. In closed-die (impression-die) forging, the top and bottom dies each carry half of the shape of the part, sunk into their faces. A few blows force hot steel to fill the cavity, and every part comes out the same.

The board drop hammer

Two upright guides 3–5 m tall stand on an anvil block of 20 times the tup. The tup, 100–1,000 kg of steel or cast iron with the top die keyed in its face, slides between them. Two or four hardwood boards (maple, beech or ash, 4–5 cm thick) wedged into the tup rise between two steel rolls turning toward each other on a belt-driven shaft. Press the treadle: the rolls grip the boards and carry the tup up; at the top a dog holds it or a trip opens the rolls, and it falls 1–2 m. One operator gives 30–60 blows a minute. Steam or air drop hammers drive the tup down as well, for heavier blows.

The forging die

  1. Blocks. Tough die steel — medium carbon with nickel, chromium and molybdenum (Alloy and Stainless Steels) — annealed soft, machined square, with a dovetail tang. Cut half the part's shape into each, by chisel, file and scraper or on a copying mill (Machine Tools), every dimension 1.5% larger than the cold part to allow for shrinkage.
  2. Draft. Give every side wall a slope (draft) of 5–7° on outside walls and 7–10° on inside walls so the forging comes out. No undercuts.
  3. Fillets. Round every corner: at least 3 mm on small parts, more on big ones. Sharp corners crack dies and fold the metal.
  4. Flash land and gutter. Around the impression, leave a narrow flat land where the dies almost meet, leaving a gap of 1.5–3 mm, about 4–5 times as wide as that gap. Outside it, cut a deeper gutter. Extra metal squirts through the land into the gutter as a thin fin (flash). The narrow land holds the metal back, so the cavity fills first.
  5. Several impressions. A die for a spanner or connecting rod usually has a fuller (thins the bar where needed), an edger (gathers metal toward the thick parts), a blocker (rough shape, generous fillets) and the finisher, side by side on the same block.
  6. Harden the die blocks to about 45–50 HRC (a file will barely mark them) by heating to about 850 °C, quenching in oil and tempering at 450–550 °C. Too hard and they crack.
  7. Trimming die. A separate punch and die in a press cuts the flash off (Presses, Punches and Dies).

Forging with it

  1. Preheat the dies to 150–250 °C with a fire laid on them; cold dies crack.
  2. Heat bar stock to 1,150–1,250 °C (bright yellow). Give one or two blows each in fuller and edger, two or three in blocker and finisher. Swab the dies between parts with oil, graphite in water or sawdust, which burns into a releasing gas cushion.
  3. Cut the forging from the bar, trim the flash while hot, then normalise or harden the batch (Steel) and tumble off the scale.

A good pair of dies makes 5,000–50,000 forgings before re-sinking. That is why drop forging only pays for parts needed by the thousand.

How to tell it worked

  • Hammer. Strike a lead block: the print should be even, not deeper on one side. A power hammer gives single soft taps on light treadle, full blows on full treadle, and stops up when you let go.
  • Drop forging. The part fills every corner; the flash is thin and even all round; there are no folds or laps. A polished section etched in dilute acid shows flow lines following the shape of the part.

Note Troubleshooting. Anvil face dents → face soft: it never hardened, or was over-tempered. Reheat the top, harden and temper again. Face chips at the edges → too hard or edges too sharp. Temper it to straw, radius the edges. Power hammer hits soft at full speed → belt slipping (tighten or dress it), spring too stiff for the ram, or dies set too high. Forging not filling corners → too cool, not enough metal in the blocker stage, or flash land too wide open; move metal toward the thick parts in the edger. Folds or laps → enlarge the fillets in the blocker. Die cracking → dies not preheated, too hard, or sharp corners in the impression.

Dangers

Danger Crushing. A power hammer, steam hammer or drop hammer will crush a hand in a fraction of a second and cannot be stopped mid-blow. Never put any part of your body between the dies. Hold work with long tongs. Lift your foot clear of the treadle whenever you are not striking, and block the ram or tup up with a hardwood block or steel prop whenever you change dies or work on the machine. A board drop hammer can slip its catch: never reach under a raised tup.

Danger Flying metal. Thin hot scraps, flash and scale can shoot from between dies at bullet speed. Thin or cold work, or a forging struck off-centre, can be flung across the shop. Wear eye protection and a leather apron, and keep everyone out of the line of the dies. Never strike cold metal or a hardened tool on a power hammer: it can shatter.

  • Anvils crush feet. Move them with a bar through the hardy hole and two people, or a hoist. Never strike a bare anvil face with a sledge or hardened hammer: chips fly off both.
  • Steam. Water trapped above a steam piston can blow the cylinder cover off; always drain first.
  • Noise. Power hammers deafen within years. Plug your ears with wax and wool.

What this unlocks

With a heavy hammer, a smithy turns blooms and puddled balls into bar and plate (Sheet Metal and Rolling), forges large axles for Wagons and Carriages and Railways, crankshafts for the The Steam Engine and The Internal Combustion Engine engines, anchors and chain links for ships, and big hand tools (Hammers, Pliers, Wrenches and Screwdrivers, Axes, Chisels, Knives and Planes). Closed-die forging makes spanners and pliers, connecting rods, gear blanks (Gears) and bicycle parts (The Bicycle) in quantity, and the same die-making skills carry into Presses, Punches and Dies.

How it was first done

The first anvils were stones. Roman smiths worked on plain iron blocks set in stumps, with separate horn stakes. Anvils with horn and heel appear in medieval Europe, and the London pattern became standard in England in the 18th and 19th centuries, made by firms such as Mousehole Forge near Sheffield and Peter Wright. In 1847 Mark Fisher in New Jersey began casting iron anvils with steel faces.

Water-powered trip hammers were pounding grain in China by the 1st century AD, and were later used there for iron; in Europe, water-driven forge hammers spread from the 12th and 13th centuries. James Nasmyth in Manchester sketched the steam hammer in 1839 and patented it in 1842; the French ironworks at Le Creusot built one, from his idea, slightly earlier. American gun factories developed drop forging with closed dies in the mid-1800s to make interchangeable lock and frame parts. Small belt-driven spring hammers, such as the Little Giant made in Minnesota from the early 1900s, put power hammers into ordinary village blacksmith shops.

Source: content/entries/metals/anvils-and-power-hammers.md