Part 7 · Home and Daily Life
Pots, Pans and Kettles
How to make the metal pots and pans of a kitchen — cast-iron cauldrons, pots, Dutch ovens, skillets and griddles; hammered and spun copper and steel saucepans, frying pans and woks, and how to line copper with tin; kettles, teapots and coffee pots; baking trays and bread and cake tins; steamers; the pressure cooker and its safety valve; trivets and pot hooks — and how to season and care for them.
- Difficulty
- ●●●●●
- Time
- A day to forge a frying pan; two to three days to raise a copper saucepan; a foundry day for a batch of cast pots once patterns are made; an afternoon for a baking tin
- Steps from zero
- 22 prerequisites →
This unlocks
Cooking and RecipesThe full path from nothing — 22 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- The Kiln
- Pottery
- Hides and Leather
- Bricks
- The Wheel and Axle
- Firebrick and Refractories
- Bellows
- Gears
- Iron (the Bloomery)
- Copper Smelting
- The Waterwheel
- The Blast Furnace and Cast Iron
- Blacksmithing
- Sheet Metal and Rolling
- Pots, Pans and Kettles
Do them roughly in this order. See it on the tech tree →
Why it matters
A clay pot cracks if heated too fast or knocked, and heats slowly (Kitchen and Cooking). A metal pot can sit in the flames for twenty years. Metal lets a cook fry hot, sear meat, boil water in minutes, bake bread in a closed pot on an open fire, and steam and stew at once. Thin metal saves fuel; heavy iron holds heat and evens out a ragged fire. Cookware is also the first thing a new foundry or sheet-metal shop can sell to every household, and it teaches thin-wall casting, raising, spinning, seaming, tinning and pressure-vessel design.
How it works
Spreading heat. A pan must carry heat sideways from where the fire touches it, or the food burns in one spot and stays raw in another.
| Metal | Conducts heat (copper = 100) | In the kitchen |
|---|---|---|
| Copper | 100 | Fast, very even; must be tinned inside against acid food |
| Aluminium | 60 | Light, even; dents (Aluminium) |
| Cast iron | 13 | Slow to heat, holds heat; heavy; cracks if dropped or quenched |
| Carbon steel (sheet iron) | 13 | Thinner and lighter than cast iron, unbreakable; hot spots |
| Stainless steel | 4 | Never rusts; needs a copper or aluminium base to spread heat (Alloy and Stainless Steels) |
A thin, poor conductor gives hot spots. The cure is thickness or copper: copper 2–2.5 mm thick, or iron 3–5 mm, cooks evenly.
Seasoning. Fat spread very thin on hot iron oxidises and links into a hard, slippery black film bonded to the metal. It keeps water off the iron and food off the pan. The method is in Kitchen and Cooking.
Tin linings melt at 232 °C: never heat a tinned pan empty. Food or water in it holds it far below that.
Pressure. Raise the pressure in a pot by 1 bar and water boils at about 120 °C: food cooks roughly three times faster, and — held there long enough — even bacterial spores are killed (Canning and Bottling).
What you need
| Job | What | Chapter |
|---|---|---|
| Cast pots, ovens, skillets, griddles | Furnace, moulding sand, wooden patterns and core boxes, flasks | The Blast Furnace and Cast Iron, Metal Casting |
| Forged pans and woks | Iron or mild steel sheet 1.5–3 mm, forge, a hollowed stump | Sheet Metal and Rolling, Blacksmithing |
| Raised copper pans and kettles | Copper sheet 1–2.5 mm, raising hammers, steel stakes | Copper Smelting |
| Spun pans | A continuously turning lathe, wooden formers | The Lathe, Machine Tools |
| Tinning, seams | Tin, rosin or sal ammoniac; brazing spelter; rivets | Tin and Pewter, Soldering and Brazing |
| Tins and trays | Tinplate or sheet iron 0.4–0.8 mm, snips, folding bars, wire | Sheet Metal and Rolling |
| Pressure cooker | Heavy pot, machined lid, rubber seal, valve weight | Boilers and Pressure Vessels, Rubber |
Cast-iron pots and pans
Casting a thin pot
Read Metal Casting first; a thin hollow vessel is a skilled foundry job.
- Patterns. Turn or carve a wooden pattern of the pot's outside, split in two halves with draft (a slight taper) on every face, plus legs and handle lugs. Make a core box — a hollow the shape of the pot's inside.
- Walls 4–6 mm, even everywhere, every inner corner rounded. Thinner and the iron chills white and brittle; uneven and it cracks as it cools (The Blast Furnace and Cast Iron). Allow 1 % shrinkage.
- Core. Ram the core box with sand bound with clay or flour paste, vent it with a wire, and bake it dry.
- Mould. Ram the pattern halves in a two-part flask, draw them, and set the core. Cast mouth-down: pour through a gate in the centre of the base, and let the legs act as risers that feed shrinking metal and let gas out.
- Pour grey iron hot and fast — white-yellow, running like water. Cool in the sand for several hours.
- Fettle: knock out the core, break off the gate, grind the fins, wire-brush, and season at once.
Big round cauldrons are often swept in loam with a profile board turning on a post, like a bell (Metal Casting).
The pots
- Cauldron: a round-bellied pot on three legs 8–12 cm long that stand steady in the embers, with two ears on the rim and an iron bail for hanging. From 5 litres for a household to 50–200 litres for washing, scalding or Soap-making.
- Iron cooking pot: flat-bottomed with a lid and side lugs, for a stove or range (Cooking Ranges, Iceboxes and Vacuum Flasks). A useful set is 2, 4 and 8 litres.
- Dutch oven: a heavy lidded pot 25–35 cm across and 10–12 cm deep, on three short legs, with a flat lid with a raised rim 2–3 cm high that holds glowing coals. Heat from below and above bakes bread, cakes and roasts on an open fire. For about 180 °C in a 30 cm oven, set a ring of coals underneath and about twice as many on the lid; check after 20 minutes. Lift the lid with a hooked iron lid lifter.
- Skillet: a shallow pan 20–30 cm across, 5 cm deep, walls 4–5 mm, a 15–20 cm handle and two pouring lips. Old skillets stood on legs in the embers.
- Griddle: a flat plate 6–8 mm thick, 25–40 cm across, with a bail or handle, for flatbreads, oatcakes and pancakes (Grain, Flour and Bread). It can be poured open in a levelled sand bed.
Judging cast ware. Hung from a finger and tapped, it should ring; a dull clack means a crack. Look inside for sand holes (small pits) and cold shuts (wrinkled seams where two streams of iron met but did not fuse). Filled with water and stood on dry stone for an hour, it must leave no damp mark. It should not rock on a flat stone.
Warning Never pour cold water into a hot cast-iron pan or set it hot on wet stone: the sudden shrinking can crack it across.
Hammered and spun pans
Forged frying pan and wok
A frying pan is 24–30 cm across with sloping sides 4–5 cm high, so steam escapes and food browns. A wok is a round-bottomed bowl 30–40 cm across and 9–12 cm deep for fast frying over a fierce, narrow flame: the hottest point is the middle, and cooked food is pushed up the cooler sides.
- Cut a disc of mild steel or wrought iron: 1.5–2 mm for a wok, 2–3 mm for a frying pan (finished base plus twice the side height plus 1 cm).
- Sink it: anneal (bright red, cool slowly) and hammer it into a shallow hollow in the end grain of a big stump, in rings from the centre out. A wok is sunk all over into a smooth bowl; a frying pan only at the edge, then its base is flattened on the anvil and its sides turned up over a stake.
- Planish: go over the whole surface with light, overlapping blows of a polished hammer on a smooth stake, to even and stiffen it.
- Handle: forge one from 10 × 20 mm bar with a three-hole end plate and rivet it on, peening the rivets inside (Nails, Rivets and Wire Fasteners). A wok gets two loop handles or a long hollow handle with a wooden grip.
- Blue and season: heat the bare pan until it turns blue-grey, then season it (Kitchen and Cooking).
Good pan: lies flat; handle does not rock on its rivets; no thin spots; black and smooth after seasoning.
Raising a copper saucepan
A saucepan is a deep pan with straight sides and one long handle: 14–22 cm across, 8–12 cm deep, holding 1–4 litres.
- Cut a disc of copper 1.5–2.5 mm thick, about the base diameter plus twice the height: 38 cm for a pan 18 cm across and 10 cm deep. Raising crowds metal inward, so the wall keeps about the sheet's thickness.
- Anneal: heat to dull red, just visible in shade, and quench (Copper Smelting). Do this whenever the copper turns hard and springy — after every pass.
- Mark the base circle with dividers.
- Raise in courses. Hold the disc tilted on a smooth, rounded raising stake with the base line just over the stake's edge. Strike just beyond the point of contact, turning the disc a little after each blow, round and round, then a ring further out, to the rim. Anneal. Repeat 6–10 courses until the wall stands upright.
- Planish the walls on a smooth stake with a polished hammer, in overlapping rows, until the surface is an even pattern of small facets. This work-hardens and stiffens the pan.
- Trim the rim level and roll it over a 3–4 mm wire.
- Handle: a cast or forged iron handle (iron passes heat poorly, so the grip stays cooler) with copper rivets.
- Tin the inside (Tin and Pewter). Re-tin when copper shows over an area as big as a thumbnail.
Seamed work. Coppersmiths also made pans and kettles from a rolled band with a cramp seam — interlocking teeth cut in both edges, closed and brazed with brass spelter at a red heat. Brazed seams survive a pan boiling dry; soft-soldered seams do not. Use soft solder only where the metal can never get hotter than boiling water.
Spinning
With a lathe that turns continuously — a treadle with a heavy flywheel, or a line shaft (Machine Tools) — pans can be spun. A disc of copper, brass, aluminium or soft steel is clamped against a wooden former turned to the pan's inside shape. At 600–1,200 turns a minute, the spinner levers a polished, round-nosed steel bar about 50 cm long against a pin in the tool rest and presses the disc onto the former in long sweeps from the centre out, greasing it with tallow or soap and annealing copper between passes. A skilled spinner makes a saucepan body in minutes, all alike.
Kettles, teapots and coffee pots
- Kettle: a closed vessel of 1.5–3 litres with a lid, spout and overhead handle, of tinned copper, tinplate, sheet iron or cast iron. The spout leaves the body low down and its tip must rise higher than the fullest water level, or it spills when filled. Braze the spout and seams; wrap the handle in cane. A whistle is a cap with two facing plates 3–4 mm apart, each pierced with a 3 mm hole.
- Teapot: best in stoneware or porcelain (Stoneware and Porcelain), or pewter or silver-plate. Three details make it work: a strainer of 15–30 holes of 2–3 mm through the wall behind the spout; a spout tip at or above the rim; and a tiny vent hole in the lid so air enters as tea pours, which stops dribbling. A 1-litre pot serves four to six cups; use one level spoon of tea per cup.
- Coffee pot: the simplest is a tall pot in which coarse-ground coffee is boiled for a minute, then left four minutes to settle. A drip pot is better: an upper chamber whose floor is a plate pierced with hundreds of 0.5–1 mm holes. Use medium-ground coffee, about 60 g per litre, and water at 90–96 °C, which drips through in 4–6 minutes. A cloth or Paper filter on the plate gives a cleaner cup.
Baking trays, bread tins and cake tins
These are folded from tinplate or sheet iron 0.4–0.8 mm thick without cutting the corners, so they hold batter and fat without solder.
- Lay out a rectangle: the base plus twice the side height each way. A loaf tin with a 20 × 10 cm base and 7 cm sides needs 34 × 24 cm.
- Fold up the sides on the folding bars (Sheet Metal and Rolling). The spare metal at each corner forms a triangular dog-ear; fold it flat against the end wall.
- Rivet or solder the dog-ears down and wire the top edge.
| Tin | Size |
|---|---|
| Baking tray | 40 × 30 cm, edges 1–2 cm; 3 cm clearance to the oven walls all round |
| Large loaf tin | 23 × 13 cm top, 7 cm deep — about 900 g of dough |
| Small loaf tin | 18 × 9 cm top, 6 cm deep — about 450 g of dough |
| Round cake tin | 20–23 cm across, 6–8 cm deep; a loose bottom or a springform band with a lever clip lets the cake out |
Round tins are a rolled band with a folded bottom, like the bucket in Sheet Metal and Rolling. Grease and flour every tin. Dry tinplate in the warm oven after washing, or it rusts.
Steamers
- Metal steamer: a tinplate or copper pan whose floor is punched with 4–5 mm holes 1–2 cm apart, made to nest in the pot's mouth 3–5 cm above the water. Stack two or three under one lid.
- Bamboo steamer: a ring of thin bamboo or wood strip 3–4 cm deep, steam-bent and pegged (Steam-Bending Wood), with a floor of slats 5–8 mm apart and a woven lid that lets a little steam escape so drops do not fall on the food. Set it in a wok over 3–4 cm of boiling water.
Keep the water topped up: a soldered steamer that boils dry comes apart.
The pressure cooker
A pressure cooker is a small boiler. At 1 bar above air pressure (about 120 °C) beans cook in 25–35 minutes instead of 2–3 hours, and it doubles as a steriliser (Sterilising Instruments and Dressings) and, if it holds the jars and you follow the times in Canning and Bottling exactly, a canner for low-acid food.
- The pot: cast aluminium 4–5 mm or steel 3 mm thick, 20–25 cm across, 4–8 litres, with a turned-in rim.
- The lid must be impossible to lift under pressure: lugs on its edge slide under the pot's turned-in rim when it is turned (a bayonet lock), or a bridge and central screw clamps it down.
- The seal: a ring of natural rubber in a groove in the lid (Packing, Gaskets and Seals). Replace it when it hardens or cracks.
- The weighted vent: a short pipe through the lid with a smooth, sharp-edged bore of 2–3 mm and a loose weight sitting on its top. The weight lifts when pressure × hole area = weight: in practice, grams ≈ 10 × pressure in bar × hole area in mm². A 3 mm hole (7 mm²) needs about 70 g for 1 bar.
- The second release: a safety plug of soft rubber that blows out at about 2 bar if the vent blocks; without rubber, a second weighted vent set at 1.5 bar, where food cannot reach it.
- Test it full of cold water, pumped to twice the working pressure, as for a boiler. Nothing may leak or bulge.
Using it: fill no more than two-thirds (half for beans and grains, which foam). Heat with the vent open until steam blows freely for a minute, put on the weight, and turn the fire down once it rocks gently; time from then. Afterwards let it cool or run cold water over the lid. Clear the vent with a wire after every use.
Trivets and pot hooks
- Trivet: three legs of 8–10 mm rod, 10–15 cm long, forge-welded or riveted to a ring 15–25 cm across, to hold a pan over coals. Three legs never rock. A low table trivet stands under hot pots on a wooden table.
- Pot hook: an S of 8–10 mm round iron about 15 cm long, ends tapered and turned up, to hang a bail from a chain or crane. Hooks of several lengths, or the toothed trammel, set the pot's height. A fireplace crane — an iron arm hinged on two pins in the fireplace wall — swings the pot out of the fire for stirring, so the cook never reaches over flames.
Care: wash iron and steel in hot water, dry over the fire and wipe with fat; never scour tin linings with sand; dry tinplate at once.
How to tell it worked
A cast pot rings, holds water and sits level. A fried egg slides on a seasoned pan with a smear of fat. A kettle filled to its fill line does not spill; a teapot pours without dribbling. Bread comes cleanly out of its tin. A pressure cooker's weight rocks steadily on a small fire.
Note Troubleshooting. Cast pot pitted → damp sand or poor venting. Cracked in the mould → uneven walls or a core too hard to give; make cores crumbly. Wall white and brittle → too thin or poured too cold. Copper cracks while raising → anneal after every course. Tin lining dull and lumpy → copper dirty or too cool; re-scour and heat until the tin flows. Seasoning sticky → too much fat; flakes → laid on dirty or rusty metal. Kettle leaks after boiling dry → soft solder melted; braze the seams. Pressure cooker leaks round the lid → seal hard or dirty, or rim dented.
Dangers
Danger Pressure cookers can explode. A blocked vent turns one into a bomb that throws boiling food and a heavy lid across the room. Never fill above two-thirds, clean the vent every time, keep a working second release, never weigh the vent down to cook faster, and never open it until the pressure has gone. Test new or repaired cookers with water at twice the working pressure, never with steam.
- Copper and lead: keep copper tinned; use pure tin for linings and lead-free solder inside any vessel (Lead).
- Burns and scalds: iron handles get as hot as the pan; use a dry cloth or mitt (Kitchen Utensils and Gadgets). Turn handles inward, away from children. Open lids away from your face.
- Molten iron: see The Blast Furnace and Cast Iron and Metal Casting. Fat fires: a lid or wet sack, never water (Kitchen and Cooking).
- Sheet edges cut: wire or fold every edge.
What this unlocks
Good pots make the kitchen range worth building, and large-scale Canning and Bottling, Soap, cheese and brewing possible. The pressure cooker brings steam sterilisation to clinics without an autoclave. Raising and spinning lead to reflectors, instrument cases and brass instruments.
How it was first done
Bronze cauldrons were cast in Shang China more than 3,000 years ago, and the Romans used bronze saucepans and frying pans much like ours. Chinese founders were casting thin iron pots from about the 5th century BC. In 1707 Abraham Darby of Coalbrookdale, who had studied Dutch brass foundries, patented casting iron pots in dry sand, and cheap pots and "Dutch ovens" spread to every household. Denis Papin showed his "digester", the first pressure cooker, with the first known safety valve, in London in 1679; home pressure cookers became common in the late 1930s. Aluminium pans, spun or pressed from sheet, appeared in the 1890s, soon after the Hall–Héroult process made the metal cheap (Aluminium).
Source: content/entries/home/metal-cookware.md