◆ Rebuild

Part 5 · Cloth and Clothing

Raincoats, Oilskins, Umbrellas and Rubber Boots

How to keep rain off people — straw and palm rain capes, oilskins painted with linseed oil, waxed cotton, rubberised Macintosh cloth, and the raincoats, ponchos and sou'westers made from them; rubber wellington boots and galoshes; and the umbrella and parasol, with their ribs, stretchers, runner and springs.

Difficulty
●●●●●
Time
A straw rain cape in two days; an oilskin in two to three weeks of drying; waxed cotton in an afternoon; a rubber-cloth coat or pair of boots in a week once you have rubber; an umbrella in three to five days
Steps from zero
10 prerequisites →

You need first

RubberMaking ClothesOils and Pressing

This unlocks

—
The full path from nothing — 10 steps before this one
  1. Cordage and Rope
  2. Stone Tools
  3. Sulfur
  4. Simple Machines
  5. Farming from Seed
  6. Spinning and Weaving Cloth
  7. Rubber
  8. Oils and Pressing
  9. Sewing, Needles and Thread
  10. Making Clothes
  11. Raincoats, Oilskins, Umbrellas and Rubber Boots

Do them roughly in this order. See it on the tech tree →

Why it matters

Being wet is dangerous as well as miserable. Wet clothes lose most of their warmth, and a person soaked in a cold wind at 5 °C can die of hypothermia in a few hours (Surviving Cold and Heat). Farmers, fishermen, shepherds and builders must work in rain; dry clothing lets them do it safely.

Rainwear also teaches three tricks of waterproofing used all through this book: shedding water off overlapping layers, as a thatched roof does; filling the pores of cloth with oil or wax; and coating it with rubber. The same skills make tents (Tents, Sleeping Bags and Camping Gear), oilcloth (Linoleum, Oilcloth and Floorcloths) and balloon envelopes (Balloons).

How it works

  • Shedding. Water runs downhill. Layers that overlap downward — straw in a cape, shingles on a roof, the upper panel of a coat lapped over the lower — let it run off without ever finding a way in. Every seam on rainwear must point downhill.
  • Filling the pores. Water creeps through the tiny gaps between threads by capillary action — the pull that draws water into a sponge. Coat the fibres with oil or wax and water beads up and runs off. Drying oils (Oils and Pressing) set into a rubbery film; wax stays soft and can be renewed.
  • A continuous skin. Rubber has no pores at all. It is the most waterproof, but it traps sweat.
  • The catch: sweat. A working person gives off a litre or more of water vapour a day through the skin. A fully waterproof coat holds it in, and it condenses inside. Good rainwear is loose, with vents, and worn over wool, which stays warm when damp (Wool).
PLAIN CLOTHOILED OR WAXEDRUBBERISED water creeps throughthe gaps between threads fibres coated, gaps filled;water beads and runs off a skin with no pores at all;it also traps sweat RIGHT: UPPER PANEL LAPS OVER LOWERWRONG: LOWER LAPS OVER UPPER upper panel outside,lower panel tuckedbehind it: water runsover the joint and ondown the outside outside(rain) lower panel outside:water running downthe upper panel dropsinto the gap and soaksthrough the seam outside(rain)
Fig. 1 Three ways to make cloth keep out rain. Plain cloth lets water creep through the gaps between threads; oil or wax coats the fibres and fills the gaps; rubber lays a continuous skin over them. Below: a seam on rainwear must lap downhill, so water running down the outside never meets an open edge.

What you need

Item For Notes
Straw, sedge, palm fibre Rain capes Long, dry, unbroken stems
Tightly woven cotton or linen, 150–350 g/m² Proofed cloth, canopies Cotton, Flax, Hemp and Linen, The Loom
Boiled linseed oil Oilskins About 1 litre per 4–5 m² for three coats
Beeswax, linseed oil, pine resin Waxed cotton Beekeeping; about 300 g per jacket
Rubber, sulfur, solvent Rubber cloth, boots Rubber, turpentine or naphtha (Ether, Acetone and Solvents, Coal Tar Chemicals)
Split bamboo or cane, hardwood, brass wire, spring steel Umbrellas Basic Woodworking, Iron and Brass Wire, Springs

Where to find it

  • Straw: rice, wheat or rye straw, cut long. Sedges and rushes from marshes.
  • Palm leaf and palm fibre: the brown, hairy fibre that wraps the trunks of fan palms such as the windmill palm, and leaves of fan and coconut palms in warm lands.
  • Bamboo: straight 2–4-year-old culms (stems) with long gaps between the joints. Rattan cane in the tropics; straight hazel or willow rods elsewhere (heavier).
  • Rubber: rubber trees and other latex plants (Rubber).

Method 1: A straw or palm rain cape

The oldest rainwear is a small thatched roof worn on the shoulders: the Japanese mino of straw or sedge and the Chinese suoyi of palm fibre. It needs no cloth, sheds heavy rain, and lets sweat out freely.

  1. Make a neck cord: a two-ply cord 1.5 m long (Cordage and Rope).
  2. Tie bundles: take a pencil-thick bundle of straw 60–80 cm long, fold the top 10 cm over the cord, and bind it tight with a twist of straw or twine. Push it hard against the last. Fill 50–60 cm of cord: this is the top row.
  3. Twine rows: 10–12 cm below, twine a second cord across the first layer (Baskets and Containers), adding a new bundle at every twist, so the second row overlaps the first by two-thirds. Make 4–6 rows, each wider than the last, so the cape flares.
  4. Trim the bottom straight at hip or knee height. Tie the neck cord at the throat.

Wear it with a wide hat (Hats, Gloves, Scarves and Stockings). Palm fibre is sewn in overlapping sheets onto a cord net. Hang it to dry; never fold it wet.

Method 2: Oilskin

Oilskin is closely woven cotton or linen soaked with a drying oil that hardens in air into a waterproof film. Fishermen's yellow oilskins ("slickers") were made this way for over a hundred years.

  1. Sew the garment first, with flat-felled seams (Sewing, Needles and Thread) lapped downhill. The oil seals the needle holes.
  2. Prepare the oil. Boil raw linseed oil gently for 2–3 hours outdoors until it thickens a little (Oils and Pressing). Stir in a spoonful of yellow ochre or lampblack per litre for colour and to shield the oil from sunlight; 5–10% pine tar or resin makes it tougher.
  3. First coat. Hang the garment on a frame and rub the warm oil in with a rag until the cloth is evenly dark and wet through, then wipe off everything that does not soak in. A thick coat never dries; it stays sticky and cracks.
  4. Dry in warm, airy shade, spread out, for 3–7 days, until it is no longer tacky.
  5. Repeat two or three more times. The finished cloth is stiff, slightly shiny and smells of oil.
  6. Store it hung up, never folded tightly or piled. Renew with one thin coat each year.

Method 3: Waxed cotton

Wax stays softer than dried oil and can be put on at home in an afternoon. Waxed cotton breathes a little, folds without cracking and is easily re-proofed.

  1. Cloth: tightly woven cotton or linen canvas, 250–350 g/m² for a jacket.
  2. Dressing: melt 2 parts beeswax to 1 part boiled linseed oil (by weight) in a pot standing in a pan of hot water — never over a bare flame. A quarter part of pine resin makes it tougher. Pour it into a tin and let it set.
  3. Warm the cloth in the sun or near a stove. Rub the bar of dressing hard all over it, or brush on the melted dressing.
  4. Melt it in: pass a warm smoothing iron (Laundry and Bleaching Cloth) or a hot stone wrapped in cloth over it, or hang it for half an hour in a cooling bread oven at about 60–80 °C (hot enough to soften wax, not to scorch cloth). The whole surface should go evenly darker with no pale patches.
  5. Cure for a day hung up. Re-wax every year, and wherever it wears pale.

Method 4: Rubberised (Macintosh) cloth

  1. Make rubber cement. Masticate dry rubber until doughy and knead in its sulfur and lime (Rubber). Shred it and soak it in 6–10 times its weight of turpentine or naphtha in a closed jar for 1–3 days, stirring, until it is a smooth paste like honey.
  2. Spread it. Stretch the cloth flat on a table. Pour a line of cement along one end and draw it across with a straight wooden blade (a doctor), leaving a film thinner than a coin. Let the solvent evaporate for an hour, outdoors.
  3. Repeat 3–5 coats, to about 0.3–0.5 mm.
  4. Double texture (Charles Macintosh's original): press two coated cloths together face to face, rubber inside, and roll them hard. It is the most waterproof and the rubber is protected from wear.
  5. Cure: dust with chalk, roll it loosely round a pole with dusted paper or cloth between layers, and heat it for 1–3 hours at 130–150 °C, judged with a pinch of sulfur as in Rubber. Uncured rubber cloth goes sticky in summer and stiff in frost.

Cut and sew it, then seal every seam: brush cement over both faces of the seam allowance before sewing, and after sewing glue a 2 cm strip of rubber cloth over the stitching inside.

The raincoat

Use the coat pattern in Making Clothes, with these changes:

  • Loose: 15–20 cm more round the chest than the wearer, to fit over a jacket and let air move.
  • Length below the knee for walking; to mid-thigh for working, with waterproof trousers or a long apron below.
  • Shoulders: avoid seams across the top. Use raglan sleeves (the seam runs diagonally from armpit to neck) or add a cape — a second layer over the shoulders, open at the back.
  • Front: overlap the fronts 12–15 cm and close them with large buttons under a storm flap — a strip that covers the buttonholes (Buttons, Buckles, Hooks and Zips).
  • Collar: stand-up, 7–8 cm, with a throat tab that buttons across.
  • Cuffs: a strap and button to close them, or an inner cuff of knitted wool.
  • Vents: 4–6 metal eyelets under each arm, and a slit across the back under the cape or yoke.

The poncho

A poncho is a sheet with a hole for the head. It covers a pack too, and with grommets it becomes a groundsheet or shelter (Shelter).

  1. Cut a rectangle of proofed cloth about 140 × 210 cm.
  2. In the middle cut a slit 28–30 cm long across the short way, and bind its edges, or sew on a hood (Making Clothes) with a drawstring round the face.
  3. Hem all round and set a grommet at each corner and the middle of each long side (Buttons, Buckles, Hooks and Zips). Press studs or ties along the sides close it into sleeves.

The sou'wester

The sou'wester is an oilskin hat with a long back brim, so rain runs off behind the collar, not down the neck.

  1. Crown: six gores (curved triangles) each one-sixth of the head circumference plus 1.5 cm at the base and 16–18 cm tall, sewn into a dome. Or two side pieces and a strip.
  2. Brim: an off-centre ring — 5–6 cm wide in front, 12–15 cm at the back. Cut two layers; sew them together with 3–4 rows of stitching round the brim to stiffen it.
  3. Ear flaps and chin ties sewn inside the brim at the sides. Line the crown with flannel.
  4. Make it up in cloth, then oil or wax it.

Wellington boots and galoshes

Wellington boots are knee-high boots of rubber: unbeatable for mud, flooded fields, dairy floors and fish quays. Galoshes are thin rubber overshoes pulled over ordinary leather shoes.

Lasthardwood or plaster, inside Liningknitted cotton, cemented Upperrubber sheet 1.5–2 mm;edges overlap 10 mm Toe cap Heel stiffener Sole6–8 mm, grooved Heel2–3 cm top: calf girth + 6 cm 35–40 cm Cure on the last:2–3 hours at 130–150 °C
Fig. 2 A rubber boot built on a last. A knitted or cotton lining goes on first, then the rubber pieces with their edges overlapped and cemented; a thick sole and heel of tough rubber; a toe cap and heel stiffener. The whole boot is cured on the last.

From sheet rubber (the good way)

  1. The last. Carve a boot last of hardwood or cast one of plaster (Gypsum and Plaster of Paris) — a foot last (Footwear) with a leg 35–40 cm tall. Make the ankle no narrower than the instep girth (round heel and top of the foot) plus 2 cm, or the foot will not go in; make the top calf girth plus 6 cm.
  2. Lining. Pull on a sock of knitted cotton or thin wool cloth, cut and sewn to fit the last tightly, and brush it with rubber cement.
  3. Upper. Roll soft rubber compound (Rubber) into sheet 1.5–2 mm thick. Cut a leg piece and a vamp (foot) piece from a paper pattern taken off the last. Lay them on the cemented lining and press them down from the middle outwards with a hardwood roller to drive out air. Overlap every edge 10 mm with cement between.
  4. Reinforce: a toe cap and a heel piece of the same sheet over the upper.
  5. Sole and heel: tough soot-filled rubber (Rubber) — sole 6–8 mm, with grooves cut across it for grip, and a heel built up to 2–3 cm.
  6. Cure on the last. Dust with chalk, pack in sand in an iron box or a closed oven, and cure 2–3 hours at 130–150 °C. Cool slowly and pull the boot off.

From fresh latex (where the trees grow)

Coat a clay or wooden last with fresh latex, dry it over a smoky fire for a few minutes until it turns brown and firm, and dip again — 15–25 dips for a boot, more at the sole. Peel it off (or wash out a clay last). The rubber is uncured: keep it out of hot sun and frost, and expect it to last a season.

Galoshes

The same as boots, but low — ankle height — and thin: a 1–1.5 mm upper and a 3–4 mm sole, made on a last a little bigger than the shoe they cover. A strap or buckle at the instep stops them pulling off in mud.

The umbrella

An umbrella is a portable roof on a folding frame. It keeps head and shoulders dry without the sweat of a coat.

Ferrule Canopy8 gores, drum-tight Rib60 cm, bamboo6 × 4 mm Top notch Stretcher27 cm, joins rib 25 cmfrom the top notch Runnerslides on the shaft Top springcatches the runner open Bottom springholds it closed Shaft80–85 cm, 12–15 mm thick 19 cm Hingewire or thread CLOSED ribs folddown runner52 cm down push up
Fig. 3 An umbrella frame. The ribs hang from the top notch; each stretcher joins its rib to the runner. Sliding the runner up the shaft pushes the stretchers out and opens the ribs; a spring in the shaft catches the runner open. Sizes are for an umbrella with 60 cm ribs.

The parts

  • Shaft (stick): the handle at the bottom, the ferrule (pointed tip) at the top.
  • Top notch (crown): a collar fixed near the top of the shaft that the ribs hinge from.
  • Ribs: 8 for a cloth umbrella (Japanese paper umbrellas use 30–70 thin ones). They hold the canopy.
  • Stretchers: one per rib, hinged to the rib about two-fifths of the way down it and to the runner at the other end.
  • Runner: a sleeve that slides on the shaft. Pushed up, it drives the stretchers out and the ribs open.
  • Springs: small catches in the shaft that hold the runner open (top spring) and closed (bottom spring).
  • Canopy: 8 triangular gores of proofed cloth or oiled paper, sewn to the rib tips.

Sizes (a walking umbrella)

Part Size
Ribs 60 cm long; bamboo 6 × 4 mm, or steel
Stretchers 27 cm; hinge on the rib 25 cm from the top notch
Shaft 80–85 cm plus handle; hardwood or bamboo 12–15 mm thick
Runner travel Open: 18–20 cm below the notch; closed: about 52 cm below
Open span About 110–115 cm across
Top notch and runner Hardwood or horn, 30 mm across; runner 6–8 cm long

For other sizes, keep the same proportions: stretcher about 45% of the rib length, joining the rib at about 42% of the way down.

Step by step

  1. Shaft. A straight, dry hardwood rod or bamboo culm, with a metal ferrule on top and a handle below.
  2. Top notch. Turn a hardwood cylinder 30 mm across and 25 mm long (The Lathe) and bore it to fit the shaft tightly. Saw 8 slots round it, 4 mm wide and 12 mm deep, evenly spaced, and cut a groove round its middle through all of them. Glue and pin it 3 cm below the ferrule.
  3. Ribs. Split bamboo into strips 6 × 4 mm, keeping the hard outer skin on the outside face. Bend each into a gentle curve over a hot iron or steam (Steam-Bending Wood) so the tip droops 5–6 cm. Drill a 1.5 mm hole 3 mm from the top end, and another at 25 cm.
  4. Runner. Turn a hardwood sleeve 30 mm across and 7 cm long, bored so it slides freely on the shaft. Cut 8 slots and a groove at its top end, like the notch.
  5. Stretchers. Split bamboo 5 × 3 mm, 27 cm long, with a hole drilled 3 mm from each end.
  6. Hinges. Pass a ring of 1 mm brass wire through the top holes of all 8 ribs, lay it in the notch groove with one rib in each slot, and twist its ends together. Do the same for the stretchers at the runner. Join each stretcher to its rib with a loop of wire or waxed thread through the two holes, bound so it pivots but does not wobble.
  7. Springs. Cut a slot 3 mm wide and 40 mm long in the shaft just below the runner's open position. Fit a strip of spring steel 3 mm wide (Springs) pinned at its lower end, with its upper end bent outward 2–3 mm. The runner pushes it flat going up and it springs out underneath; press it to close. Put a second spring where the runner rests when closed. (A simpler catch: a peg through a hole in the shaft.)
  8. Canopy. Open the frame and measure from tip to tip of neighbouring ribs (about 45 cm). Make a paper triangle with two sides the rib length and that base, and add 1 cm seam allowance on each side and 2 cm for the hem. Cut 8 gores, all lying the same way on the cloth so they stretch alike. Sew them together with flat seams, hem the edge, and make a small hole at the centre.
  9. Fit. Slip the canopy over the ferrule. Sew each seam's lower corner firmly to its rib tip (fit a small brass or horn cap over each tip first), and tack each seam to its rib at the middle with a few stitches. The cloth should be drum-tight when open; if it sags, unpick the tips and take in the gores. Bind a cloth rosette tightly round the shaft over the top hole.
  10. Proof the canopy with wax, oil or rubber (above) unless the cloth is tight enough to shed rain alone.

Paper umbrellas. In China and Japan, umbrellas with many fine bamboo ribs are covered with strong mulberry paper (Paper) glued to every rib, then brushed with a drying oil — tung, perilla or linseed — and dried in the sun. They are light and cheap but tear in strong wind.

The parasol

A parasol keeps off sun, not rain. Make it the same way but lighter — 6–8 ribs of thin bamboo or cane, 45–55 cm long — with a canopy of pale cotton, linen, silk or oiled paper, which reflects heat. It prevents sunburn and heat exhaustion in the midday sun (Surviving Cold and Heat).

How to tell it worked

  • The bucket test. Make a bag of a scrap of the proofed cloth, hang it up and fill it with water. Good oilskin and rubber cloth hold water for a day with no drip; waxed cotton for several hours.
  • The beading test. Water poured on the cloth forms round beads and rolls off.
  • The wear test. Walk an hour in steady rain and check shoulders, seams, cuffs and collar from inside.
  • Heat and cold. A piece left in hot sun must not go tacky; crumpled after a frost, it must not crack.
  • The umbrella opens and closes in one movement, stays open in a moderate wind, and the runner catches every time.

Note Troubleshooting. Oilskin stays sticky for weeks → oil not boiled, coats too thick, or dried in cold damp air. Wipe it hard with a rag and dry it warm. Oilskin cracks at folds → too many coats, or stored folded. Hang it; next time use thinner coats. Wet at the seams → seams not lapped downhill, or not sealed. Re-wax or tape them. Wet all over the inside, cloth looks fine → condensation, not leakage. Add vents; wear wool underneath. Rubber cloth sticky or smelly → undercured. Cure again. Boot splits at the overlap → air trapped or no cement. Roll seams from the middle outward. Umbrella turns inside out → ribs too thin or stretchers too short; make them stiffer, or tie the tips together loosely with a cord between ribs.

Dangers

Danger Oily cloth can catch fire by itself. Rags, cloth and garments soaked in linseed oil heat up as the oil hardens and can burst into flame hours later. Dry oilskins hanging open in the air, never folded or in a heap. Spread used rags flat outdoors to dry or burn them at once (Oils and Pressing).

Danger Solvents and rubber cement burn fiercely. Turpentine and naphtha vapour is heavier than air and flows to any flame. Mix and spread rubber cement outdoors, far from fires and lamps (Ether, Acetone and Solvents). Curing rubber gives off hydrogen sulfide, a poison gas (Rubber).

  • Sweat chills. Hard work in a sealed coat soaks you from inside; then stopping in the cold can bring on hypothermia. Open the vents, take layers off before you sweat.
  • Rubber boots do not keep feet warm. Wear thick wool socks and dry boots and socks every night; feet left wet for days get trench foot — numb, swollen, rotting skin. Never wade deep water in boots or waders; once they fill, they drag you under.
  • Umbrellas and lightning. In a thunderstorm in open country, do not hold up an umbrella with a metal shaft or ferrule; crouch low away from trees (Reading the Weather). Rib tips poke eyes in crowds — fit rounded tip caps.

What this unlocks

How it was first done

Capes of straw, grass and palm fibre are very old; the Japanese mino and the Chinese suoyi were still worn in the 20th century. Sailors tarred their canvas coats — hence "Jack Tar" — and later painted them with linseed oil. The Olmec, Maya and Aztec peoples of Mexico used rubber long before Europeans; by the 1820s, rubber overshoes made by dipping clay moulds in latex in Pará, Brazil, were being shipped to Boston by the thousand.

In Glasgow in 1823 Charles Macintosh patented a cloth of two layers stuck together with rubber dissolved in coal-tar naphtha, a waste of the gasworks; Thomas Hancock of London had found how to soften rubber by mastication, and the two firms joined. The coats were stiff in winter and sticky in summer until vulcanisation (1839–1844) cured them. In 1853 the American Hiram Hutchinson bought a licence from Goodyear and began making rubber boots in France; the North British Rubber Company of Edinburgh followed in 1856 and made over a million pairs for soldiers in the trenches of the First World War. The name comes from the Duke of Wellington's leather boots of the 1810s.

Parasols were carried in ancient Egypt, Assyria and China. A collapsible umbrella with jointed ribs was made in China by the first century AD, and oiled-paper umbrellas spread from there to Japan and Korea. In London in the 1750s Jonas Hanway carried one in public and was jeered by coachmen, who feared for their trade. In 1852 Samuel Fox in England introduced the light steel rib of U-shaped section that umbrella frames still use.