◆ Rebuild

Part 3 · Metals

Molybdenum

A soft, grey, greasy-looking ore that people long mistook for graphite holds a metal that melts at 2,623 °C. Roast the ore to a white oxide, reduce it in hydrogen to powder, press and sinter it like tungsten, and work it hot into wire and foil for lamps, valves and furnace windings. The same metal makes steel tough and deep-hardening, and the raw ore, cleaned and ground, is one of the best lubricants there is.

Difficulty
●●●●●
Time
A week to concentrate and roast the ore; two days from oxide to a sintered bar; days more to work it into wire or foil. MoS2 grease takes an afternoon once you have clean concentrate.
Steps from zero
31 prerequisites →

You need first

Tungsten and Filament WireSulfuric Acid

This unlocks

—
The full path from nothing — 31 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Salt
  14. Lime
  15. Fermentation
  16. Lye and Potash
  17. Glass
  18. Bellows
  19. Saltpeter
  20. Copper Smelting
  21. Iron (the Bloomery)
  22. Laboratory Glassware
  23. Sulfuric Acid
  24. Blacksmithing
  25. The Battery
  26. Steel
  27. Electrolysis
  28. Copper Wire
  29. Iron and Brass Wire
  30. Hydrogen, Oxygen and Gases
  31. Tungsten and Filament Wire
  32. Molybdenum

Do them roughly in this order. See it on the tech tree →

Why it matters

Molybdenum is tungsten's easier younger brother. It melts at 2,623 °C (tungsten at 3,422 °C), weighs about half as much (10.2 g per cm³ against 19.3), and works hot at a lower heat. Once you can make Tungsten and Filament Wire, you can make molybdenum in the same furnaces. It gives you:

  • Foil and wire that seal into glass and quartz. Molybdenum expands with heat nearly as much as hard glass, and rolled thin it seals into Fused Quartz and Halogen Lamps, which is how every halogen lamp is closed.
  • Supports, grids and mandrels for lamps and radio valves, and the hooks that hold a tungsten filament.
  • Furnace windings that run at 1,600–1,700 °C in hydrogen, far hotter than nichrome (Electric Kilns and Furnaces, Very-High-Temperature Furnaces).
  • Better steel. A quarter of a percent of molybdenum makes a steel harden right through a thick shaft and stay tough after tempering. A few percent makes stainless steel resist salt water. In high-speed tool steel it can replace most of the scarce tungsten (Alloy and Stainless Steels).
  • A lubricant. The ore itself, molybdenum disulfide, is a slippery grey powder that keeps sliding metal apart under crushing loads and in vacuum, where oil and graphite fail.

How it works

The ore is a sulfide. Nearly all molybdenum comes from molybdenite, molybdenum disulfide (MoS₂, 60% molybdenum). It is built of sheets — molybdenum between two layers of sulfur — that slide over each other at a touch, which is why it feels greasy and lubricates.

Roast, then reduce. Heated in air, the sulfur burns off as sulfur dioxide and leaves molybdic oxide (MoO₃), a white powder that turns yellow while hot:

molybdenum sulfide + oxygen → molybdic oxide + sulfur dioxide.

The oxide is then stripped of its oxygen by hydrogen, exactly as for tungsten, in two stages: first to a brown lower oxide, then to grey metal powder. 1 kg of oxide gives 667 g of metal and needs about 470 litres of hydrogen, in practice three to five times that flowing through.

Two traps to remember. Molybdic oxide melts at 795 °C and gives off a white vapour well below that, from about 650–700 °C. Too hot, and the oxide fuses into a glassy lump or smokes away. And hot molybdenum metal burns in air above about 500 °C, with the same white smoke, so every hot step for the metal happens in hydrogen, or in air only for seconds.

Hot work makes it tough. Like tungsten, sintered molybdenum is brittle until it has been hammered and drawn, which stretches its grains into fibres. Heat worked molybdenum above about 1,100 °C for long and the grains grow round again and it turns brittle. So anneal it only at 800–900 °C, enough to relieve stress but not to recrystallise.

What you need

Item For See
Molybdenite concentrate, 85–95% MoS₂ Feed Below, Ore Dressing: Jigs, Tables and Flotation
Iron roasting pan or brick hearth; ammonia water, filters and dishes Roasting, purifying Finding and Identifying Ores, Ammonia
Hydrogen, dried, 1–2 m³ a day Reduction, sintering, hot work Hydrogen, Oxygen and Gases
Hydrogen tube furnace, press and mould, sintering bell Powder and bars Tungsten and Filament Wire, Powder Metallurgy
Rotary swager, small rolling mill, draw bench with carbide and diamond dies Wire and foil Tungsten and Filament Wire, Iron and Brass Wire, Sheet Metal and Rolling
Strong Sulfuric Acid Drying hydrogen; catching roast gas

Where to find it

  • Molybdenite — soft (a fingernail scratches it), flaky, lead-grey with a bluish tinge and a bright metallic shine on fresh flakes. Flakes bend but do not spring back. It marks paper like a pencil. It hides in quartz veins in and around granite, often with tin and tungsten ores, and as fine specks scattered through huge bodies of shattered granite-like rock with copper ore. Weathered outcrops sometimes show a canary-yellow crust (molybdic ochre).
  • Molybdenite or graphite? Graphite is the usual confusion. Molybdenite is twice as heavy (4.7 times water against 2.2), bluer, and on the glazed surface of a pot it leaves a greenish-grey streak where graphite leaves black. Heat a flake on a knife tip in a flame: molybdenite smells of burning sulfur and grows a white-yellow crust; graphite does neither.
  • Wulfenite — lead molybdate. Thin, square, plate-like crystals of a striking orange, honey-yellow or red-brown, with a greasy-glassy shine and very heavy for their size. Found in the weathered, rusty upper parts of lead deposits (Lead). A smaller ore, but easy to see.
Molybdenite molybdenum disulfide, the ore Graphite carbon, the look-alike Bluish lead-grey, bright on fresh flakes Black to steel-grey, duller Streak on glazed pottery: greenish-grey Streak on glazed pottery: black same size, same balance 4.7 times as heavy as water 2.2 times as heavy as water Heated: sulfur smell, white-yellow crust Heated: no smell, no crust
Fig. 1 Telling molybdenite from graphite. Both are soft, grey and greasy and mark paper. Molybdenite is twice as heavy, bluer, smells of sulfur when heated, and leaves a greenish streak on glazed pottery.

Concentrating. Most molybdenite ore holds well under 1% of the mineral, so it must be concentrated. Molybdenite is one of the few minerals that is naturally water-repelling: ground fine and stirred with water, a drop of paraffin oil and a frother, its flakes climb onto air bubbles and float off as a grey froth while quartz sinks. This is froth flotation, described in Ore Dressing: Jigs, Tables and Flotation. Float it several times over to reach 85–95% MoS₂. In small, rich quartz veins you can also hand-pick it.

Step 1: Roasting to oxide

1 Concentrate85–95% MoS₂, floated 2 Roast 550–650 °Cdull red; sulfur dioxide off 3 Purifyammonia, or sublime 4 Pure oxidewhite MoO₃ 5 Hydrogen, 600 °Cturns brown (MoO₂) 6 Hydrogen, 1,000 °Cgrey metal powder 7 Press and sintercurrent, in hydrogen 8 Swage, draw, rollwire and foil
Fig. 2 From ore to wire. Concentrate is roasted below 650 °C to technical oxide, purified by ammonia or by subliming, reduced in hydrogen in two stages to grey powder, pressed and sintered into a bar, and worked hot into wire and foil.
  1. Spread the dry concentrate 2–3 cm deep in an iron pan or on a brick hearth with the fire beside it, so hot air sweeps over the top (Finding and Identifying Ores).
  2. Light and hold at 550–650 °C, a dull red just visible in a shaded room. Burning sulfur feeds the roast, so watch it does not run away: if patches glow bright cherry or white smoke rises, rake them open and cut the fire.
  3. Rake every 15–30 minutes so fresh surfaces meet the air and no crust forms.
  4. Finish. After 6–12 hours the flakes have become a powder, lemon-yellow hot and pale grey-green to white cold, that no longer smells of sulfur when reheated. It weighs 90% of the concentrate.
  5. Catch the gas — sulfur dioxide — up a tall chimney, or better into a lead chamber or contact tower to make Sulfuric Acid.

The result is technical oxide, 85–90% molybdic oxide with the rock waste still in it: good enough for steel (below). For wire and foil, purify it.

Step 2: Pure oxide

Method A, through ammonia (like tungsten):

  1. Stir the technical oxide into warm ammonia water (about 10%), 1 kg to 4–5 litres. The oxide dissolves as ammonium molybdate; iron oxide, quartz and most dirt stay behind.
  2. Let settle and filter. A blue liquid carries copper: recrystallise twice.
  3. Evaporate slowly until white crystals form, and pour off the last liquid with its impurities.
  4. Calcine the crystals in a clean pottery dish at 400–500 °C (just below a visible glow) for an hour. Ammonia and water leave; a white to very pale yellow-green powder remains: pure molybdic oxide.

Method B, by subliming. Heat technical oxide in a fireclay tray in a muffle at 1,000–1,100 °C (bright orange), with a slow draught of air over it and out through a long, cool flue. The oxide boils off as white smoke and settles in the flue as soft, white, feathery crystals, over 99% pure; the dirt stays in the tray. It needs no chemicals at all.

Step 3: Reducing to powder

Use the hydrogen tube furnace of Tungsten and Filament Wire, with the same purging, pop test and burn-off flame at the exit.

  1. Load boats with oxide only 1–2 cm deep.
  2. First stage: 550–650 °C for 2–4 hours. The white oxide turns chocolate- to violet-brown (molybdenum dioxide). Do not go hotter until this is complete, or the oxide fuses into a glassy cake that hydrogen cannot get into.
  3. Second stage: 950–1,100 °C for 2–4 hours. The brown turns to an even dull grey metal powder.
  4. Cool in hydrogen. Fine hot molybdenum powder catches fire in air.
  5. Weigh. First stage loses 11% of the oxide weight; complete reduction loses 33.3%. Anything less, the powder is not done.

Step 4: Bars

  1. Press the powder in a split steel mould at 1.5–3 tonnes per cm², as for tungsten. Bars 10–15 mm square and 30–60 cm long are usual in industry; start with 6 × 6 × 150 mm.
  2. Presinter in hydrogen at 1,100–1,200 °C for an hour, so the bar can be handled.
  3. Sinter, either by current in the hydrogen bell of Tungsten and Filament Wire, at about 90% of the current that melts a test bar, for 15–20 minutes; or by heating in a hydrogen furnace at 1,800–2,000 °C for 4–8 hours, if you have one wound with tungsten. The bar shrinks 10–15% each way and reaches about 9.5–9.8 g per cm³, 93–96% of solid metal.

A good bar rings when struck, shows a fine, even, silvery-grey grain where a scrap end is snapped, and has no cracks along its length.

Molybdenum wire

  1. Swage hot. Heat the bar in hydrogen to 1,200–1,400 °C (yellow to bright yellow) and swage it (Tungsten and Filament Wire describes the rotary swager), 10–15% reduction in area per pass. Work quickly: a few seconds in air is harmless, but a bar that smokes white is burning. Lower the heat as it thins, to about 900–1,000 °C (bright orange) by 2–3 mm.
  2. Draw warm. Below about 2 mm, coat the wire with colloidal graphite and draw it at 400–700 °C (from no glow to dull red), heated by a small gas flame just before a heated die (Iron and Brass Wire). Carbide dies take it to about 0.3 mm, diamond dies finer.
  3. Clean off the graphite by passing the wire through molten caustic soda or hot Lye and Potash with a current, then rinse.
  4. Stress-relieve coils at 800–900 °C in hydrogen for 10–15 minutes. Never higher.
Use Diameter
Lamp filament supports and hooks 0.15–0.4 mm
Mandrel for coiled-coil tungsten filaments 0.05–0.3 mm
Grids of radio valves 0.05–0.15 mm
Furnace winding 1–2 mm
Glass-sealing lead-ins 0.5–1 mm

A test: good wire bends round its own diameter and back without cracking, and its surface is a bright, even silver-grey. Wire that snaps short with a sugary-looking break has been overheated and recrystallised.

Mandrel wire. A tungsten coil wound on molybdenum wire, then coiled again, makes the compact coiled-coil filament. The molybdenum is then dissolved away in a warm mixture of nitric and sulfuric acid (about 1 part strong nitric, 1 part strong sulfuric, 2–3 parts water by volume), which eats molybdenum but leaves tungsten untouched.

Glass seals. Molybdenum expands about 5 millionths of its length per °C, close to hard borosilicate sealing glasses (Scientific Glassblowing and Glass-to-Metal Seals). Heat the wire red so it forms a thin oxide skin and wet it at once with the hot glass. A good seal looks golden-brown through the glass; a black or grey one is over-oxidised and will leak.

Molybdenum foil

  1. Flat-roll a 1–2 mm wire, or a hot-forged strip, between polished steel rolls (Sheet Metal and Rolling). Start hot (600–900 °C, flushing the rolls' bite with hydrogen or working fast), then warm, and finish cold for the last passes. Anneal at 800–900 °C in hydrogen between groups of passes.
  2. Lamp foil: 0.02–0.03 mm thick, 2–5 mm wide, 8–15 mm long.
  3. Feather the edges. Etch the strip briefly in the hot nitric–sulfuric mixture, or electrolytically in lye, so that its edges become knife-thin. A square edge cracks the quartz; a feathered edge bends with it.

How it is welded to the tungsten filament and pinched into quartz is in Fused Quartz and Halogen Lamps. A good foil is bright, flat and free of pinholes when held against a lamp.

The molybdenum-wound furnace

Tapped transformer start low, raise slowly hot zone 30–40 cm, 1,600–1,700 °C Dry hydrogen Hydrogen fills the case Burn-off flame vent flame Alumina powder insulation Molybdenum winding 1.5 mm wire, about 6 m Alumina work tube 5–8 cm bore Steel case gas-tight, gaskets The winding must never meet air while hot.
Fig. 3 A molybdenum-wound tube furnace. Molybdenum wire is wound on an alumina tube and buried in alumina cement and powder inside a gas-tight steel case. Hydrogen flows through the case and the work tube and burns at the exits. A tapped transformer starts the cold winding at low voltage.

This furnace reaches 1,600–1,700 °C, enough to sinter carbide and alumina, fire zirconia, and melt and refine small samples of steel and nickel alloys.

  1. The tube. A dense alumina tube (Alum and Alumina), 5–8 cm across inside and 60–80 cm long. Fireclay and quartz do not last: hydrogen attacks silica at these heats.
  2. The winding. Wind 1.5 mm molybdenum wire evenly round the middle 30–40 cm, turns about 1 cm apart, slightly closer at the ends of the hot zone (where heat leaks away). Bed it in a thin paste of fine alumina and a little water. About 6 m of wire gives 4 kW.
  3. The case. Pack the tube in fine alumina powder or bubble alumina inside a welded steel case with gas-tight end plates and gaskets, the terminal rods coming out through insulated, water-cooled glands.
  4. The gas. The winding must never meet air while hot. Feed a steady stream of dry hydrogen (or cracked ammonia, 75% hydrogen and 25% nitrogen, Ammonia) into the case, and burn it at a small vent. Purge before every heating.
  5. The power. Molybdenum's resistance rises about nine times from cold to 1,600 °C. Cold, this winding is about 0.17 ohm; hot, about 1.6 ohm at 80 volts and 50 amperes. So start at a quarter of full voltage, from a The Transformer with tappings or a saturable reactor, and raise it step by step over an hour as the winding warms.

Treated so, a winding lasts hundreds of firings; one that sees air while hot smokes away in minutes.

Molybdenum in steel

You do not need to make pure metal for steel. Molybdenum oxide is easily reduced by molten iron, and molybdenum does not burn out during steelmaking. So:

  • Simplest. Press technical oxide with a little lime and tar into briquettes and drop them into the molten steel in an The Electric Arc Furnace or crucible, under the slag, early in the melt. About 95% of the molybdenum goes into the steel. For 0.25% molybdenum in 100 kg of steel you need 375 g of oxide (250 g of metal).
  • Ferromolybdenum, a lump alloy of 60–70% molybdenum with iron, is handier for big works. Technical oxide mixed with iron scale, aluminium powder (Aluminium) and ferrosilicon, in a sand-lined pit, is lit with a magnesium ribbon (Magnesium); it burns violently for a minute or two and leaves a lump of alloy under a crust of slag.
Steel Molybdenum What it does
Chromium–molybdenum ("chrome-moly") 0.15–0.3%, with about 1% chromium Hardens right through shafts, axles, bolts, gears, pressure vessels and bicycle frames; stays tough after tempering (Pressure Vessels and Valves)
Molybdenum high-speed steel 5–9%, with tungsten, chromium, vanadium Cuts as well as tungsten high-speed steel with half the tungsten. One part of molybdenum does the work of about two of tungsten.
Stainless 2–3% Resists pitting by salt water, brine and acids (Corrosion and Its Prevention)
Heat-resisting and creep steels 0.5–1% Boiler tubes and steam pipes that must not stretch slowly when hot (Boilers and Pressure Vessels)

The full story of alloy steels, and how to make them, is in Alloy and Stainless Steels.

Molybdenum disulfide lubricant

Cleaned and ground, natural molybdenite is one of the best solid lubricants known. It carries loads that squeeze oil out completely, and works in vacuum and dry gas, where graphite does not (graphite needs moisture to slide). Above about 350–400 °C in air it slowly burns to oxide.

Cleaning and grinding

  1. Start with your best concentrate, floated at least three times. Every grain of quartz left in it is an abrasive that will scour the bearing.
  2. Leach it in hot, dilute Hydrochloric Acid (1 part strong acid to 5 of water) for an hour, stirring, to dissolve limestone and iron oxides. Wash with water until the washings are no longer sour.
  3. Grind wet in a porcelain or flint-lined jar mill with water or spirit for 24–48 hours (Ball Mills, Crushers and Grinders). The flakes split into finer flakes.
  4. Settle and pour off (Abrasives and Grinding Stones describes settling). Stir the slurry into a tall jar of water, wait one minute, and pour off the cloudy upper part into a second jar; the quartz and coarse grains sink fast and are left behind. Let the second jar stand overnight and collect the grey sludge.
  5. Dry below 120 °C. Store sealed.

Test: rub a pinch between finger and thumb. It should feel like soft soap with no grit at all, and leave your skin a shiny blue-grey. Rubbed on glass with a fingertip, it should not scratch.

Using it

  • Dry film. Rub the powder hard onto oil-free metal with a leather pad until it is a shiny, dark blue-grey. For screws, slides and locks that must not collect dirt, and parts in vacuum.
  • Molybdenum disulfide grease. Make lime grease (Bearings and Lubrication): warm 10 parts tallow or oil and stir in 1 part slaked lime (Lime) as a milk, cooking gently until the water is gone. Off the heat, stir in 3–5% by weight of molybdenum disulfide (up to 10% for slow, heavily loaded joints) and mix until it is an even grey-black. Use it on heavily loaded slow joints: kingpins, splines, press slides, tractor pivots.
  • Anti-seize paste. Stir 50–60% of molybdenum disulfide into a heavy oil or tallow until it is a thick paste. Smear it on bolts, studs and press-fitted parts that must come apart again after years of heat and rust.

Good grease is smooth, even in colour, and does not separate after a week in the jar; slid between two steel plates under hard pressure it feels slippery, with no scratching sound.

How to tell it worked

  • Roast is pale, odourless when reheated, and 10% lighter; pure oxide is white (green or blue tints mean partial reduction or copper); powder is even grey and a third lighter than the oxide.
  • Bar rings; wire bends round its own diameter; foil is bright and pinhole-free.
  • Steel: quench 40 mm bars of plain and chrome-moly steel, cut them and file the faces from edge to centre. The plain one goes soft a few millimetres in; the alloy stays hard much deeper (Forge Shops and Heat Treatment).

Note Troubleshooting. Roast fused into glassy lumps → above about 700 °C. Roast thinner, rake more, keep the fire back. White smoke in the reduction tube → first stage too hot. Hold 550–650 °C until all is brown. Yellow or brown patches in powder → incomplete reduction. Thinner layers, drier hydrogen, more time. Wire splits or snaps → worked too cold, or overheated. Swage hotter early; never anneal above 900 °C. Furnace winding failed → air leaked into the case. Check gaskets; keep hydrogen flowing. Grease scratches → grit. Settle the disulfide more thoroughly.

Dangers

Danger Hydrogen explodes when mixed with air, and every hot step here runs in hydrogen. Purge, test, keep a positive flow, burn off the exhaust, and work in a high, airy building (Tungsten and Filament Wire, Hydrogen, Oxygen and Gases).

Danger Sulfur dioxide from roasting chokes and burns the lungs. Roast in the open or under a tall chimney, stand upwind, and stop if your throat burns.

  • Ferromolybdenum making throws molten metal and burns far hotter than any furnace. Only in the open, lit from a distance, behind a wall, never near water or damp ground.
  • Molybdenum oxide dust and fume irritate the lungs and eyes. Handle powders damp or in closed vessels and wear a damp cloth mask.
  • Pyrophoric powder. Fine hot molybdenum powder catches fire in air: cool it under hydrogen.
  • Hot acids for mandrel and foil etching give off brown, poisonous nitrogen fumes. Work outdoors or under a hood.
  • Heavy currents in sintering and furnace windings: take off rings, switch off before touching clamps.

What this unlocks

Halogen lamps (Fused Quartz and Halogen Lamps), coiled-coil filaments (The Light Bulb), valve grids (The Vacuum Tube), hot hydrogen furnaces and molybdenum disilicide elements (Very-High-Temperature Furnaces, Powder Metallurgy), base plates for power diodes (Power Electronics and Motor Drives), deep-hardening and stainless steels (Alloy and Stainless Steels), and grease for heavy machines (Bearings and Lubrication, The Tractor). Its salts give the molybdate test for phosphate (Identifying Substances) and are a trace fertiliser for clover and beans (Chemical Fertilisers).

How it was first done

For centuries molybdenite, graphite and galena were all sold as molybdaena, from the Greek word for lead, and used for pencils. In 1778 the Swedish chemist Carl Wilhelm Scheele showed that molybdenite was a separate mineral: boiled with nitric acid it gave a white "earth", molybdic acid, quite unlike anything from graphite. In 1781 his friend Peter Jacob Hjelm reduced that oxide with carbon and linseed oil to the first grains of the metal.

It stayed a curiosity for a century. In 1891 the Schneider works at Le Creusot in France made the first molybdenum steels, and around 1910 William Coolidge's methods for ductile tungsten at General Electric were turned to molybdenum wire for lamp supports and valve grids. The great deposit at Climax, Colorado, worked from 1918 with froth flotation, made molybdenum cheap; by the 1930s and 40s molybdenum high-speed steels were replacing tungsten ones in America. Molybdenum disulfide came into wide use as a lubricant in the 1940s. In 1959 Edward Zubler and Frederick Mosby at General Electric built the tungsten-halogen lamp, sealed with molybdenum foil into quartz.

Source: content/entries/metals/molybdenum.md