◆ Rebuild

Part 12 · Transport

Boats and Sails

How to build a boat from planks instead of a single log — clinker and carvel planking, caulking, keel and rudder — and how to make it go with the wind, even against it, using a sail of woven cloth and a few ropes. Plus anchors to hold it still.

Difficulty
●●●●●
Time
Two to three months for a first 5 m sailing boat, with two or three people
Steps from zero
4 prerequisites →

You need first

Basic WoodworkingCordage and RopeSpinning and Weaving Cloth

This unlocks

Diving and Underwater WorkHarbours and LighthousesLife Jackets, Lifebuoys and LifeboatsSteamships
The full path from nothing — 4 steps before this one
  1. Stone Tools
  2. Cordage and Rope
  3. Basic Woodworking
  4. Spinning and Weaving Cloth
  5. Boats and Sails

Do them roughly in this order. See it on the tech tree →

Why it matters

A dugout canoe can only be as big as the biggest tree (Rafts and Canoes). A boat built of planks has no such limit: join enough planks along a strong backbone and you can build a fishing boat, a river barge, or a ship that carries 50 tonnes across the sea.

A sail turns that boat into a machine powered by the wind, for free, for as long as the wind blows. A sailing barge with a crew of three can move as much grain, stone or timber as a hundred porters, and it needs no road. For most of history, every big city stood on a river or a coast for exactly this reason. Sailing ships carried the trade, the ideas and the crops that tied distant peoples together.

This chapter builds a small, open, wooden boat about 5 m long that can be rowed or sailed — the kind of boat that served fishermen everywhere for a thousand years — and explains how the same methods scale up.

How it works

The hull

The hull floats for the same reason a canoe does: it pushes aside its own weight of water (see Rafts and Canoes). A plank hull is built around a keel — a long, strong timber down the middle of the bottom, like a backbone. At the front it joins a curved stem, at the back a sternpost. The planks wrap from stem to stern on both sides, and curved frames (ribs) inside hold them in shape.

Speed. A hull pushing through the water makes a wave at its bow and another at its stern. As it speeds up, the bow wave grows longer until the boat is sitting in a hollow between its own two waves; going faster means climbing its own bow wave, which takes enormous power. That limit, the hull speed, is roughly

speed in km/h ≈ 4.5 × √(waterline length in metres)

A 5 m boat tops out near 10 km/h; a 20 m ship near 20 km/h. Long boats are fast boats.

The sail

There are two ways a sail drives a boat:

  1. Pushing. With the wind behind you, it simply blows on the sail. Easy, but only takes you downwind.
  2. Lifting. When the wind blows across the boat, a curved sail works like a bird's wing: the air flowing around its curved back pulls on it. The force is roughly sideways and a little forward. The boat's keel, deep in the water, resists being pushed sideways — just as a knife blade resists being pushed flat-side through butter but slides easily edge-first. The only way left for the boat to go is forward.

This is how a sailing boat travels across the wind and even towards it, at an angle. A square sail can manage about 60–70° from the wind; a fore-and-aft sail (one set along the length of the boat) about 45°. To reach a place straight upwind, you tack: zigzag at 45° first to one side, then the other.

POINTS OF SAIL TACKING UPWIND WIND No-go zone about 45° each side of the wind Close-hauledsail pulled in hard Beam reachfastest Broad reach Runningsail across, wind behind Start Goalstraight upwind Tackbow turnsthrough the wind Tack
Fig. 1 Points of sail, seen from above. No sail can drive a boat straight into the wind (the shaded zone); to reach a point upwind, the boat zigzags, turning its bow through the wind at each corner.

Balance

The push of the wind acts at the middle of the sail (its centre of effort). The resistance of the water acts at the middle of the underwater hull (its centre of lateral resistance). If the sail's centre is far behind the hull's, the stern is blown away and the boat keeps turning into the wind; too far forward and it keeps turning away. Set the mast so the boat turns very slightly into the wind when you let go of the tiller. That is safe: a boat left alone then turns into the wind and stops.

What you need

Part Material Size for a 5 m boat
Keel Oak, one straight piece 5 m long, 10 cm wide, 12–15 cm deep
Stem and sternpost Oak, from naturally curved branches 10 cm square
Planks Oak, larch, pine or cedar, split or sawn 12–14 planks, 1.5–2 cm thick, 15–20 cm wide, 5–6 m long (join shorter ones with long scarfs)
Frames Oak "crooks" (curved branches) or steamed ash or oak 12–16 pieces, 4 × 5 cm, every 40–50 cm
Fastenings Iron or copper nails with roves (washers), or wooden pegs (treenails) 600–1,000 nails for a clinker boat
Caulking Tarred wool, animal hair, moss or hemp fibre; pine tar and pitch A few kilograms; see Tar, Pitch and Glue
Mast Straight spruce, pine or fir pole 4.5–5 m, 8–10 cm thick at the foot
Sail Tightly woven linen, hemp or wool cloth 8–10 m²
Rope Hemp or flax, 8–12 mm About 60 m
Rudder and tiller Oak plank and ash 1 m × 30 cm rudder blade
Oars Ash or spruce 2.5–3 m each, two pairs

Tools: axes and an adze (Axes, Chisels, Knives and Planes), a saw (Files and Saws), an auger or bow drill for holes, chisels, a plane, a hammer, a light anvil or iron block for riveting, wedges, clamps (or wooden wedges and rope), and a steam box (below).

Where to find it

  • Oak is the classic boat timber: strong, rot-resistant and it bends well when steamed. For planks, choose a straight trunk free of knots and split it lengthways like a cake — radially, from the bark to the heart. Riven planks follow the grain, so they do not split; this is how the Vikings got 15–20 planks from one oak log. See Basic Woodworking.
  • Crooks. Where a big branch leaves the trunk, the grain flows around the curve. Cut these naturally curved pieces from felled oaks and keep them: they make frames, stems and knees that are far stronger than pieces cut across the grain.
  • Pine, spruce and fir grow tall and straight in cold climates and on sandy soils — they make masts, spars and oars. Choose a young tree grown in a crowded stand, so its trunk is straight and has small branches.
  • Caulking fibre. Sheep's wool, cattle hair, sphagnum moss from bogs, or old rope picked apart into loose fibres (called oakum once soaked in tar).
  • Sailcloth is woven linen (Flax, Hemp and Linen), hemp or wool (Wool) — see Spinning and Weaving Cloth and The Loom. Heavy canvas and long ropes are made as in Ropewalks and Sailcloth.

Method 1: Clinker building (planks overlapping)

In a clinker (or lapstrake) boat, each plank overlaps the edge of the plank below by a few centimetres, like the boards on a shed wall, and the overlaps are riveted together. The planks build up a shell first; the frames go in afterwards. It is light and strong, and the best method for a first boat.

CLINKER: PLANKS OVERLAP CARVEL: PLANKS EDGE TO EDGE outsideinside outsideinside Nail head Rovewasher, nail endhammered over it Lap 2.5 cmtarred wool between Plank1.5–2 cm thick Rivet every12–15 cm along the lap;frames fitted afterwards Caulkingfibre driveninto a V seam Pitchpoured over Treenailoak peg, 2.5 cm,wedged at the end Frameset up first,every 30–45 cm Plank3–10 cm thick
Fig. 2 Two ways of planking, seen in cross-section. Clinker: the planks overlap and are riveted through the lap with a nail and a rove. Carvel: the planks lie edge to edge on the frames, and the seam is packed with caulking and sealed with pitch.

The backbone

  1. Cut the keel. Hew a straight oak timber 5 m long, 10 cm wide and 12–15 cm deep. Cut a shallow groove, the rabbet, along both upper edges for the first plank to sit in.
  2. Join the stem and sternpost to each end with a long sloping joint (a scarf) at least three times as long as the timber is deep, glued with pitch, and fastened with wooden pegs or iron bolts.
  3. Set it up upright on trestles about 70 cm off the ground, brace it with props, and check with a plumb line that stem and sternpost are vertical.
  4. Make moulds. Cut three temporary cross-sectional shapes from rough boards — one for the middle, one halfway to each end. They tell you the shape of the hull. Stand them on the keel and brace them.

The planks

  1. The first plank (the garboard) sits in the rabbet next to the keel. Planks are not straight: lay a thin, cheap board in place against the moulds, mark on it where the keel edge runs, transfer this curve to the real plank, and cut. This is called spiling.
  2. Steam it to bend. At the ends, planks must bend and twist. Build a steam box (Steam-Bending Wood): a long, closed wooden box with a pot of boiling water feeding steam into one end. Steam oak 1 hour for every 2.5 cm of thickness. Take it out with gloves and bend it into place at once — you have a minute or two. Clamp it and leave it to cool.
  3. The next plank overlaps the first by about 2.5 cm. Plane a narrow bevel along the top edge of the plank below so the two sit flat on each other, and tapering more sharply near the stem and stern so the planks close into a smooth line there.
  4. Rivet the lap. Every 12–15 cm along the overlap, drill a hole through both planks. From outside, drive an iron or copper nail through. Inside, put a small square or round washer of iron (a rove) over its point, push it down with a hollow punch, cut the nail off 3 mm above the rove, and hammer the end over into a little rivet head while a helper holds a heavy iron block against the nail head outside. See Nails, Rivets and Wire Fasteners.
  5. Repeat plank after plank, both sides alternately so the hull stays symmetrical, until you reach the top edge (the sheer). A 5 m boat has 6–7 planks a side.

Finishing the hull

  1. Fit the frames. Remove the moulds. Bend steamed ash or oak ribs, or fit carved crooks, against the inside of the planks every 40–50 cm, and rivet or peg each one to every plank it crosses.
  2. Fit the gunwale (a thick strip along the top edge), seats (thwarts), and blocks with holes for the oars.
  3. Seal and paint. Paint pine tar, or tar thinned with linseed oil, on the whole hull inside and out (Tar, Pitch and Glue, Pigments, Paints and Varnish).

Method 2: Carvel building (planks edge to edge)

For bigger vessels, builders put the frames up first on the keel, like the ribs of a skeleton, and then nail planks to them edge to edge, giving a smooth hull. Carvel planking is easier to repair and suits large ships and heavy planks of 4–10 cm.

  1. Set up the keel, stem and sternpost as above.
  2. Raise a frame every 30–45 cm. Each frame is made of several curved pieces (futtocks) overlapping and pegged together.
  3. Fasten each plank to every frame with two treenails — pegs of dry oak about 2.5 cm thick, driven into tight holes and wedged at both ends — or with iron spikes.
  4. Leave each seam slightly open on the outside, in a narrow V about 3 mm wide at the outer surface.
  5. Caulk the seams (below).

Caulking

Caulking fills the gaps between planks so water cannot pass.

  1. Twist the fibre. Roll a loose strand of oakum, hemp fibre, tarred wool or moss between your palm and your thigh into a thread as thick as a pencil.
  2. Drive it in. Lay it along the seam and drive it in with a blunt, wedge-shaped iron or hardwood caulking iron and a wooden mallet, a little at a time, in loops, then flatten it tight. A well-caulked seam rings when struck rather than thudding.
  3. Pay the seam. Pour or brush hot pitch along the top of the caulking to seal it (Tar, Pitch and Glue).

In a clinker boat, a strand of tarred wool or hair is laid between the planks as each lap is riveted.

Tip A new boat leaks. Dry wood shrinks; wet wood swells. A newly built boat, or one that has been out of the water all summer, leaks at every seam for the first day or two. Keep it in the water (sunk in the shallows if necessary) and the seams close. Never caulk a dry boat so tight that the swelling planks have no room — they can buckle or spring their fastenings.

Rudder and keel

The rudder. The oldest way to steer is a big oar over the side near the stern. The Viking steering oar hung on the right-hand side — the "steer-board" side, still called starboard. Better is a stern-hung rudder: a flat oak blade hung on the sternpost by two or three iron hinges (pintles — pins — on the rudder that drop into gudgeons — rings — on the sternpost). A wooden tiller, about 1–1.2 m long, fits into its top. Push the tiller to the left and the boat turns right.

Keels and leeboards. For sailing, the boat must grip the water sideways. A deep-keeled boat does this by itself. A flat-bottomed barge or punt does not: fit leeboards, wide pear-shaped boards about 1.5 m long and 60 cm wide pivoted on each side. Lower the one on the side away from the wind; raise it when going downwind or in shallow water. Dutch barges sailed this way for centuries.

Ballast. A small sailing boat needs weight low down to resist being blown over. Stow 50–150 kg of stones in bags in the bottom near the middle, tied in so they cannot slide.

Sails and rigging

Mast4.5–5 m spruce or pine Yardspar the sail hangs from Halyardpull to raise the sail Shroudholds the mast up Reef points Stem Keelgrips the water sideways Ballaststones, low and central Sail8–10 m², linen or hemp Sheetsets the sail's angle Tillerpush left to turn right Pintles andgudgeons Rudder
Fig. 3 A small boat with a lug sail. The yard hangs from the mast on the halyard; the sheet controls the angle of the sail; shrouds hold the mast up sideways. Underwater, the keel resists sideways drift and the rudder steers.

The best first rig is a lug sail: a four-sided sail hung from a sloping wooden spar (the yard) that is hoisted up the mast. It is cheap, strong, easy to make, needs few ropes, and sails well. The spritsail (held out by a diagonal pole) and the triangular lateen of the Mediterranean are also good.

The sail

  1. Cloth. Use the tightest-woven, heaviest cloth you can make — linen or hemp at about 400 g per square metre is ideal; wool works (Viking sails were wool, sometimes coated with fat). Loose cloth lets the wind through.
  2. Cut the panels in strips running down the sail, overlapping each other by 2–3 cm, and sew each seam with two rows of stitching (Sewing, Needles and Thread).
  3. Hem all edges twice, and sew a bolt rope — rope about 10 mm thick — all round the edge. The rope takes the strain, not the cloth.
  4. Corners. Sew triangular patches of extra cloth into each corner and work a strong eyelet (a ring of rope sewn into a hole) for the ropes.
  5. Reef points. Sew a row of short ties across the sail about a quarter of the way up. In strong wind you lower the sail a little and tie up the bottom part (reef knots), making it smaller: this is reefing.
  6. Proof it. Traditional working sails were "barked" — soaked in a hot brew of oak bark or tree bark with red ochre and fat — which preserves them against rot.

The rigging

  • Mast. Stand it in a mast step — a block of oak fixed on the keel with a square hole for the mast foot — and through a hole in a strong thwart. Set it about a third of the boat's length from the bow for a lug sail.
  • Shrouds. Two ropes from near the top of the mast to each side of the hull, a little behind the mast, hold it upright.
  • Halyard. A rope from the yard, over a smooth hole or a wooden pulley (a block, see Simple Machines) at the masthead, and down to the deck. Haul it to raise the sail.
  • Sheet. A rope from the back lower corner of the sail to the stern. Pull it in to flatten the sail across the wind; let it out to spill the wind.
  • Tack. A short rope holding the front lower corner of the sail down near the mast.

Sailing

  1. Learn in a gentle, steady breeze of 10–20 km/h (leaves and small branches moving, a few small waves with no white crests), on a lake or sheltered bay, close to shore and with the wind blowing toward the shore.
  2. To stop, point the boat into the wind and let the sheet go. The sail flaps and the boat drifts to a halt.
  3. With the wind behind, let the sheet right out until the sail is square across the boat.
  4. With the wind from the side, pull the sheet in until the sail just stops flapping at its front edge. Let it out a little at a time until it starts to flap, then pull it back in just enough. This is the fastest point of sail.
  5. Toward the wind, pull the sheet in hard and steer as close to the wind as you can while the sail stays full. If the sail flaps, turn away a little.
  6. Tacking. To change from one zigzag to the other, gain a little speed, then push the tiller firmly away from you. The bow swings through the wind; the sail flaps, then fills on the other side. With a lug sail, you may need to lower the yard and shift it to the other side of the mast.
  7. When the wind rises, reef early — while it is easy. If you wonder whether to reef, reef.

Anchors

An anchor holds the boat still in a bay, off a beach, or while fishing.

  • Stone anchor. A heavy, flat stone (10–25 kg for a 5 m boat) with a hole bored through it near one end, or with a groove cut round it, for the rope. It holds by weight alone and drags in a strong wind.
  • Killick. A stone held in a frame of two crossed hardwood sticks whose sharpened ends point down and dig into the bottom like claws. Much better grip than a plain stone.
  • Iron anchor. A shank with two curved, pointed arms (flukes), and a crossbar (stock) at the top set at right angles to the arms. The stock lies flat on the bottom and turns the anchor so one fluke digs in. A 5–8 kg iron anchor holds a 5 m boat. Forge it from wrought iron (Blacksmithing).

Pay out enough rope. Let out a length of anchor rope at least 5 to 7 times the depth of water. A short rope pulls upward and lifts the anchor out of the bottom. A couple of metres of chain, or a heavy stone tied just above the anchor, keeps the pull flat along the seabed.

How to tell it worked

  • Leak test. Launch the boat and leave it for two days. After the planks have swollen, it should take in no more than a few litres a day. Bail it out and mark the water level inside each morning.
  • Balance test. In a steady side wind, let go of the tiller. The boat should slowly turn into the wind. If it turns away, move the mast back or make the sail's back part bigger; if it turns hard into the wind, move the mast forward.
  • Upwind test. Pick a point straight upwind and tack toward it. A good boat gains ground steadily; if you are getting nowhere, the boat is slipping sideways.

Note Troubleshooting. Water comes in at the garboard (the plank next to the keel) → this is the commonest leak. Re-caulk the seam and check the rabbet is bedded in pitch. Planks split when nailed → drill a pilot hole first, slightly smaller than the nail, and keep nails at least 2 cm from the end of a plank. A plank cracks while bending → steam it longer, or choose straight-grained, knot-free wood. Riven wood bends far better than sawn. The boat will not sail toward the wind and slides sideways → it needs more grip in the water: deepen the keel, add leeboards, or pull the sail flatter. A baggy sail drives sideways more than forward. The boat heels (leans) too far → reef the sail, add ballast low down, and have the crew sit on the side the wind is coming from.

Dangers

Danger Capsize and drowning. Sudden gusts are the main killer of small boats. If a gust heels the boat hard, let the sheet go at once — keep it in your hand, never tie it to the boat. Everyone aboard should be able to swim. Carry a bailer, spare oars and something that floats for each person. In cold water read the warnings in Rafts and Canoes; for rescue, see Life Jackets, Lifebuoys and Lifeboats.

Danger The swinging spar. When the wind crosses behind the boat (a gybe), the sail and any spar at its foot swing across violently and can knock a person unconscious and overboard. Keep your head low when turning downwind, and gybe slowly with the sheet pulled in.

  • Offshore wind and changing weather. Wind blowing off the land carries a boat out to sea. Learn to read the sky (Reading the Weather) and stay ashore when you are unsure. Head for shelter at the first sign of a squall: a dark, low cloud bank with a sharp front, or ruffled dark water racing toward you.
  • Lee shore. A coast the wind blows onto is the most dangerous place for a sailing boat: it can be driven onto rocks with no room to turn. Keep plenty of sea room.
  • Building. Steam burns are serious — wear thick gloves and keep your face away from the box when opening it. Boats on trestles can topple; brace them well. Hot pitch sticks to skin and burns deep.
  • Shipworm. In warm salt water, small boring clams (shipworm) riddle wooden hulls in a year or two. Haul boats out regularly, keep them coated with tar, and dry them in the sun.

What this unlocks

A good boat opens the sea for Fishing and coastal trade from sheltered harbours, and far voyages once you can find your way (Navigation). Inland, boats on rivers and Canals and Locks carry the heavy goods of early industry. Add a The Steam Engine to drive paddle wheels or a propeller and you have Steamships, independent of the wind. The mast, ropes, pulleys and winches of a ship are also the tools of Cranes and Lifting and building.

How it was first done

Pictures of sailing boats on Egyptian pottery and rock art date from about 3500–3200 BC, and sails were in use on the Nile, where the wind blows upstream and the current flows down. The Khufu ship, buried beside the Great Pyramid around 2500 BC, is 43 m long, built of cedar planks sewn together with rope. By about 1300 BC, ships like the one wrecked at Uluburun off Turkey were carrying 10 tonnes of copper ingots across the eastern Mediterranean; their planks were joined edge to edge with hidden tongues locked by pegs.

Northern Europe developed the clinker boat. The Nydam boat from Denmark (about AD 320) is one of the earliest; Viking ships such as the Gokstad ship (around AD 890) carried people to Iceland, Greenland and North America. The stern-hung rudder appears in China in pottery boat models from the 1st century AD, and in Europe around 1200. In the 1400s, Portuguese and Spanish builders combined carvel planking with square and lateen sails in caravels and carracks, the ships of the first ocean voyages around Africa and to the Americas.

Source: content/entries/transport/boats-and-sails.md