◆ Rebuild

Part 3 · Metals

Nails, Rivets and Wire Fasteners

The small iron things that hold everything together — hand-forged nails, rivets, staples, pins and welded chain. Each one is simple; what matters is making thousands of them, quickly and reliably.

Difficulty
●●●●●
Time
A minute per nail once practised (a beginner, five); a few minutes per rivet; ten to fifteen minutes per chain link
Steps from zero
12 prerequisites →

You need first

Blacksmithing

This unlocks

—
The full path from nothing — 12 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)
  12. Blacksmithing
  13. Nails, Rivets and Wire Fasteners

Do them roughly in this order. See it on the tech tree →

Why it matters

Pegs, lashings and joints can hold wood together, but slowly and with great skill. A nail does it in seconds. With nails you can board a floor, close in a roof, build a door, a box, a crate, a fence or a boat in a fraction of the time. Rivets join metal to metal — the blades of shears and tongs, the handles of pots, the plates of buckets, tanks and boilers, and later the hulls of iron ships and the frames of bridges. Chain lifts buckets from wells, anchors boats, hauls logs, drags ploughs and holds gates. Pins, staples, hooks and cotters fasten cloth, fences, harness and machines.

None of these is hard to make. The challenge is quantity: an ordinary timber house needs tens of thousands of nails. For most of history, nails were made one at a time by hand, and they were valuable enough that people sometimes burned down old buildings to recover the nails from the ashes. This chapter shows how to make them quickly and well.

How it works

  • A nail holds by friction. Driven in, its wedge-shaped point pushes the wood fibres aside, and they press back hard on the shank. A square, tapered hand-forged shank grips far better than a smooth round one, and a nail driven through and bent over on the far side (clenched) holds better still — this is how doors and boat planks were nailed.
  • A rivet is a soft pin with a head on one end, pushed through matching holes in two pieces and then hammered on the other end to form a second head. The pieces are clamped between the heads. A rivet put in red-hot shrinks as it cools and pulls the pieces together even tighter.
  • A chain is a row of links, each a short bar bent into a loop and forge-welded closed (see Blacksmithing). It is only as strong as its worst weld.

All of these want soft, tough wrought iron, not steel: they must bend without cracking. Choose your best, most fibrous bloom iron. Iron containing phosphorus — common in bog ore — is cold-short: it forges well hot but snaps when bent cold. A cold-short nail breaks when you clench it, and a cold-short chain can snap without warning. Test your iron: forge a rod, let it cool, and bend it double in a vice or a crack in a log. Good iron bends flat on itself; cold-short iron cracks. Keep cold-short iron for things that are never bent or shocked.

What you need

Item Notes
Forge, anvil, hammer, tongs See Blacksmithing. A 0.6–0.9 kg hammer for nails
Nail rod Wrought iron rod 4–8 mm square, as long as you can hold (50–60 cm). Draw it out by hand, or slit it from flat bar (Sheet Metal and Rolling)
Hardy A short chisel standing edge-up in the anvil's square hole, or set edge-up in a hardwood block beside a stone anvil
Nail header A steel bar with a tapered hole: see below
Rivet set and snap Punches for closing and rounding rivets (below)
Dolly A heavy iron block or bar to hold against a rivet head
Round rod Wrought iron, 6–12 mm, for chain and staples
Fine dry sand Welding flux
Drawn wire Brass or copper wire for pins (see Iron and Brass Wire and Zinc and Brass)

Where to find it

All of this is made from iron from the Iron (the Bloomery) bloom, forged into bar. Rods are the slow part. A smith drawing rod by hand can make perhaps a few metres an hour. Historically, nail rod was made in a slitting mill, where water-powered rolls flattened a bar and then rotary cutters slit it into square rods — see Sheet Metal and Rolling. Until you have one, assign the drawing of rod to an apprentice, or work two or three rods at once in the fire.

Making a nail header

The header is a steel bar 25 mm wide, 10–12 mm thick and 30 cm long, with one end widened slightly to make room for the hole.

  1. Punch a hole through the widened end, about 1 cm from the end, slightly smaller than the rod you will use. A header for 6 mm nail rod has a hole about 5 mm across at the top.
  2. Drift the hole so that it tapers wider toward the underside. The nail shank wedges in the top of the hole, and once headed it drops out from below.
  3. Dress the top face flat and very slightly domed.
  4. Harden the end and temper it to blue, so the face resists the hammer but does not crack.

Make one header for each size of nail you need (other heading tools are in The Blacksmith's Tooling). A header with a shallow cup in its face, or a second punch with a cup in its end, makes round-headed rivets.

Method 1: The hand-forged nail

1 Point 2 Nick 3 Snap off 4 Head 5 Rosehead nail four-sided taper, quarter turn every blow or two hardy light blows cut most of the way through, 1–1.5 rod widths from the shank Header on a gap bend the rod; it breaks at the nick, leaving a stub on top one hard blow down then four slanting blows, one from each side square, tapered shank head from above
Fig. 1 Forging a rosehead nail. Point the rod, nick it over the hardy, drop it into the header, snap it off and head it with four or five blows.

For a general-purpose rosehead nail about 7 cm long, from 6 mm square rod:

  1. Heat the last 8 cm of the rod to yellow. Keep two or three rods in the fire and work them in turn.
  2. Point. Lay the end on the anvil face near the far edge and hammer it into a four-sided taper, turning the rod a quarter turn after every blow or two. The taper should run the whole length of the shank, about 6 cm, ending in a blunt chisel point. This takes 8–12 blows. Work fast; you want to finish the nail in one heat.
  3. Measure. Hold the point beside the header: the shank should go through it with about 1–1.5 rod thicknesses (6–9 mm) of full-size rod standing above the top. That stub becomes the head.
  4. Nick. Hold the rod on the hardy at that point and strike it lightly, turning it, so the hardy cuts most of the way through on all four sides. Do not cut through.
  5. Snap. Drop the point into the header, held over the anvil's hole or a gap between two stones, and bend the rod sharply to break it off at the nick.
  6. Head. Hit the stub straight down, hard, to spread it. Then give four quick slanting blows, one from each side, to make the faceted, rose-like head. Done well, this takes five blows.
  7. Release. Tap the header on the anvil edge, or hit the point from below, and the nail falls out. Let it cool in a heap on dry ground or in a box. Do not quench nails in water; they stay softer cooled in air.
  8. Back to the fire.

A practised nailer does all this in one heat, in under a minute. Your first nails will take three heats each. Make a hundred before you judge yourself.

Other nails use the same steps with different points and heads:

Nail Shape Use
Rosehead Square shank, faceted head General timber work, doors, frames
Clasp or L-head Head hammered flat to one side Floorboards: the head sinks flush
Clout Short shank, wide flat round head Roofing, fixing hide, cloth or sheet metal to wood
Spike 15–25 cm long, from 10–12 mm rod Heavy timbers, bridges, docks
Tack 1–2 cm long, sharp point, flat head Leather, upholstery, shoes
Boat or clench nail Long shank, round head, used with a rove (a small square washer) Boat planks: the point is cut off and peened over the rove like a rivet
Horseshoe nail Thin, flat, wedge-shaped head Shoeing horses: soft enough to clench outside the hoof

Using hand-forged nails.

  • Choose a nail 2½–3 times as long as the thickness of the board you are nailing down.
  • In hardwood, near the end of a board, or with large nails, pre-drill a hole about two-thirds of the shank thickness with an awl or a drill (see Drills and Boring).
  • A nail with a blunt point splits wood less than a sharp one: it crushes the fibres instead of wedging them apart.
  • To clench, drive the nail through so 1–2 cm sticks out, hold an iron dolly against the head, and bend the point over along the grain, then drive its tip back into the wood like a staple.

Method 2: Rivets

1 Rivet inhead in a cupped dolly 2 Setdraw the plates together 3 Swellflat blows on the tail 4 Round offfinish with the snap grip1½ × diameter holes match the rivet(1 mm larger if hot) rivet set:its hole fitsover the tail one or two blows closeany gap between plates the rivet swells andfills the hole tightly snap:cuppedpunch round head on bothsides; plates clamped
Fig. 2 Riveting. Set the plates together with the rivet set, swell the tail with the hammer, then round it with the snap. A rivet needs 1½ diameters of tail sticking out to make a round head.

Making rivets. Forge them like nails, but without a point: cut the rod to length on the hardy, drop it in a header of the right hole size, and form the head with a cupped punch (the snap) for a round head, or with flat blows for a flat head. Rivets must be soft: use your softest iron, or copper (see Copper Smelting) for leather, knife handles and light work. Anneal copper rivets by heating to dull red and quenching before use.

Sizes.

  • Rivet diameter: for thin sheet, about 2–3 times the sheet thickness (but at least 3 mm); for thick plate, about 1½ times.
  • Length: the combined thickness of the pieces (the grip) plus 1½ diameters for a round head, or 1 diameter for a flat or countersunk head.
  • Holes: drill or punch them the same size as the rivet for cold riveting; about 1 mm larger for hot rivets up to 20 mm.
  • Spacing: rivets at least 3 diameters apart, and at least 1½ diameters from any edge.

Cold riveting (rivets up to about 6 mm, and all copper rivets):

  1. Drill or punch matching holes; clamp or pin the pieces together.
  2. Push the rivet through from below and rest its head in a cupped hollow on the dolly or anvil, so the head is not flattened.
  3. Set: place the rivet set — a punch with a hole in its end that fits over the rivet tail — over the tail and strike it once or twice. This drives the pieces tightly together.
  4. Swell: strike the tail straight down two or three times with the flat of the hammer. This upsets the rivet so it fills the hole.
  5. Shape: work around the edge of the tail with the ball or the corner of the hammer, doming it over.
  6. Finish: put the snap over the dome and strike it to make a neat round head.

Hot riveting (larger rivets, plates, tanks and boilers) is a team job: one person heats the rivets, one (the holder-up) presses the dolly against the head, and one or two strike.

  1. Heat the rivet to bright orange to yellow.
  2. Pass it quickly into the hole with tongs; the holder-up braces the dolly against the head.
  3. Strike the tail with heavy, square blows to swell it and fill the hole, then form the head with a snap and sledge.
  4. Work fast: the whole rivet must be closed before it cools below red. As it cools it shrinks by about 1% and pulls the plates together.

For watertight seams (tanks, boilers), see Sheet Metal and Rolling for caulking.

Method 3: Staples, pins and cotters

  • Staples for fences, gates and hasps: cut 8–12 cm of 5–8 mm rod, point both ends like a nail, and bend it into a U over a round bar.
  • Cotters and split pins: a cotter is a flat tapered wedge driven through a slot to lock two parts (an axe head, a wheel on its axle, a plough beam). A split pin is a length of half-round wire bent double, pushed through a hole and its legs spread to stop it falling out. Both hold a part that must be taken apart again.
  • Hooks and eyes: bend from rod; the eye is a loop forge-welded closed if it will carry weight.
  • Pins for cloth: cut brass or copper wire 0.6–1 mm thick (see Copper Wire) into 2.5–3 cm lengths. Sharpen one end by twirling it against a fine stone. For a head, either upset the other end in a tiny header die with a light hammer, or wind two turns of finer wire round the end and hammer them tight — the way pins were headed for centuries. Brass is best: iron pins rust and stain cloth. Making pins and needles by the thousand is covered in Needles and Pins.

Method 4: Chain

1 Cut and scarf 2 Bend a U 3 Thread, close, weld 4 The chain 13–14 × rod diameter ends tapered onopposite faces over the horn or around bar, at orange heat last link scarfs overlap here:flux, welding heat,light blows, then firm inside 3½–4 × d inside 1½ × d 8 mm rod: 11 cm pieces,links 32 × 12 mm inside
Fig. 3 Making a chain link. Cut a piece about 13–14 rod diameters long, scarf both ends, bend it into a U, thread it through the last link, close it and forge-weld it.

Proportions. A strong, general-purpose link has an inside length of about 3½–4 rod diameters and an inside width of about 1½ rod diameters. Each link needs a piece of rod about 13–14 diameters long. For 8 mm rod: cut pieces 11 cm long, for links about 32 mm long and 12 mm wide inside. Make one test link and adjust the length before cutting a hundred.

  1. Cut all the pieces for the chain.
  2. Scarf both ends of a piece: upset the very ends slightly, then hammer each into a short, flat taper at an angle, the two scarfs on opposite faces so they lap neatly when the link is closed.
  3. Bend it into a U over the anvil horn or a round bar the size of the inside of the link.
  4. Thread the open U through the last finished link of the chain.
  5. Close it so the scarfs overlap.
  6. Weld. Bring it to welding heat — light yellow, with a few star-sparks — fluxed with fine sand. Most smiths put the weld on one of the long sides, where it can be hammered flat on the anvil face. Strike lightly to stick, then firmly.
  7. Shape the link on the horn so it is evenly oval and the weld is the same thickness as the rest.
  8. Repeat. Make chain in short lengths of 5–10 links, then join the lengths with one last link.

For a well-made wrought-iron chain, a safe working load is roughly 5 kg for every square millimetre of rod cross-section, counting both sides of the link. For 8 mm rod (50 mm² per side), that is about 500 kg. Never trust any untested chain.

How to tell it worked

  • Nails: drive one into seasoned oak through a pilot hole. It should go in straight and not bend; the head should not crack or fly off. Clench one: it should bend flat without cracking. Pull one out with a claw: it should resist strongly.
  • Rivets: tap the head lightly with a small hammer while resting a fingertip on the other head. A tight rivet feels solid and rings; a loose one moves or sounds dead. Cut out loose rivets with a chisel and replace them.
  • Chain: proof-test every length by hanging twice its intended working load from it for a minute, clear of everyone. Then examine every weld: any link that has stretched, opened, cracked or shows a dark line across the weld must be cut out and replaced.

Note Troubleshooting. Nail head splits or crumbles → rod too cold when heading, or the iron is red-short (contains sulfur). Head it at a bright orange heat. Nails snap when clenched → cold-short (phosphoric) iron. Use different ore, or keep that iron for things that are not bent. Nail sticks in the header → hole does not taper enough underneath, or the shank was too thick. Drift the hole larger from below. Rivet bends over instead of swelling → tail too long, or hit at an angle. Cut the tail to 1½ diameters and strike square. Plates still loose after riveting → not set together first, or holes too big. Use the rivet set before shaping the head. Chain weld opens under test → too cool, dirty fire, or scarfs too short. Clean the fire, flux, and weld at a full welding heat.

Dangers

Danger Chain and hook failures kill. A chain under load that breaks whips back and drops its load. Never stand or let anyone stand under a suspended load, or in line with a chain under tension. Proof-test every chain and hook before use, and inspect it often: stretched links, cracks and rust pits mean it must be retired.

  • Flying hot bits. The snapped-off ends of nail rod and the cut ends of rivets fly off hot. Point the hardy away from people, and keep the floor around the anvil clear.
  • Burns. Hand-forging hundreds of nails means hundreds of hot pieces. Let them cool in one place, in a metal or clay box, away from anything that burns.
  • Hot riveting. Never throw hot rivets between workers. Pass them with tongs, and wear leather over your arms and feet.
  • Eyes and ears. Rivet heads and scale can fly; wear eye protection if you can make it, and ear plugs of wax and wool for long sessions.

What this unlocks

Nails make Timber Framing and Log Building, Roofs, Furniture, doors and boats faster and stronger. Rivets build Sheet Metal and Rolling tanks, The Steam Engine boilers, Steamships, rail wagons and Steel Frames and Tall Buildings. Chain serves wells, Cranes and Lifting, anchors, the The Plough and, as roller chain, the bicycle and machine drives. Threaded fasteners come next: Screws, Nuts and Bolts.

How it was first done

Bronze rivets and pins were in use in Egypt and Mesopotamia by about 3,000 BC, and bronze nails soon after. Iron nails were made by the million in the Roman Empire: when the Roman army abandoned its fortress at Inchtuthil in Scotland around AD 87, it buried nearly 900,000 iron nails rather than leave them for the local tribes. Viking shipbuilders fastened their overlapping hull planks with iron rivets clenched over square roves. In Europe and colonial America, nailing was a cottage industry: whole families in England's West Midlands made nails by hand at home forges from rod supplied by slitting mills, from the 1600s into the 1800s. Machines that cut nails from iron sheet appeared in the 1790s, and nails made from drawn steel wire took over in the late 1800s. Pins are ancient too; in 1776 the economist Adam Smith used a pin workshop, where each worker did one of about eighteen separate operations, as his famous example of the division of labour.

Source: content/entries/metals/nails-and-fasteners.md