◆ Rebuild

Part 14 · Electronics and Computing

Making Microchips

How a chip is really made, from a crystal of silicon to a tested part with legs. Slicing and polishing wafers, printing patterns with light, etching, doping, wiring, packaging and testing, and the dust-free rooms it all happens in. The realistic road from a workshop making 10-micrometre chips to a modern factory, and why the last steps take a whole industry.

Difficulty
●●●●●
Time
A year or more to set up a 10-micrometre chip line once pure silicon and transistors exist; about a week per batch of wafers. Decades, and a nation's industry, to approach modern chips
Steps from zero
63 prerequisites →

You need first

Integrated CircuitsPure SiliconPhotographyClean Rooms

This unlocks

Flat Screens: LCD and LED DisplaysMicroprocessors and Personal Computers
The full path from nothing — 63 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. The Kiln
  10. Pottery
  11. Charcoal
  12. Hides and Leather
  13. Lime
  14. Bricks
  15. Salt
  16. Mercury
  17. Lye and Potash
  18. Fermentation
  19. The Wheel and Axle
  20. Glass
  21. Firebrick and Refractories
  22. Bellows
  23. Saltpeter
  24. The Lathe
  25. Gears
  26. Glass Fibre and Glass Wool
  27. Copper Smelting
  28. Iron (the Bloomery)
  29. Lead
  30. Laboratory Glassware
  31. Sulfuric Acid
  32. Pumps
  33. The Waterwheel
  34. Lenses
  35. Blacksmithing
  36. Gold and Silver
  37. The Blast Furnace and Cast Iron
  38. Bronze
  39. Hydrochloric Acid
  40. The Battery
  41. The Vacuum Pump
  42. Magnets
  43. Steel
  44. Chimneys, Stoves and Heating
  45. Bearings and Lubrication
  46. The Steam Engine
  47. The Light Bulb
  48. Copper Wire
  49. Electrolysis
  50. Photography
  51. Hydrogen, Oxygen and Gases
  52. Centrifugal Pumps and Fans
  53. Machine Tools
  54. The Generator
  55. The Vacuum Tube
  56. The Electric Arc Furnace
  57. Ammonia
  58. Ice and Refrigeration
  59. Pure Silicon
  60. Ventilation and Air Conditioning
  61. Semiconductors and the Transistor
  62. Clean Rooms
  63. Integrated Circuits
  64. Making Microchips

Do them roughly in this order. See it on the tech tree →

Why it matters

Integrated Circuits showed the planar process: grow glass on silicon, print a pattern on it with light, etch windows, soak in dopant, lay aluminium on top. With lines 25 micrometres (μm) wide, that gives gates, adders and a few hundred transistors. This chapter covers what comes after: making chips reliably and in quantity, shrinking them, and how today's factories actually work.

Shrinking is the whole game. Halve the width of every line and four times as many transistors fit in the same area, each faster and using less power. The first microprocessor (1971) had about 2,300 transistors with 10 μm lines. A phone chip today has tens of billions, with features a few hundredths of a micrometre across.

Be honest about the scale. A few dozen people, with the rest of this book behind them, can run a 10 μm line and make 8-bit Microprocessors and Personal Computers and memory chips. Reaching 1 μm (the chips of about 1990) needs hundreds of specialists and several supporting industries. Modern chips took the whole world sixty years; one leading factory costs more than 20 billion dollars. No town will rebuild that. A town can climb the first rungs, and know where the ladder goes.

How it works

The loop

Every chip is built by repeating one loop:

  1. Add a layer: grow it (oxide), lay it down from a gas (polysilicon, glass), or coat it on (metal, resist).
  2. Print a pattern on it with light through a photomask (lithography).
  3. Remove or change material where the pattern says: etch it, or put dopant into it.
  4. Clean away the resist and every trace of dirt.

A first chip goes round the loop four to six times. A modern processor goes round 60–100 times, in over a thousand steps, taking three to four months from bare wafer to finished chips.

How small can light print?

smallest line ≈ k × wavelength ÷ NA

NA (numerical aperture) measures how wide a cone of light the lens gathers: about 0.1 for a simple lens, up to 0.93 for the best lenses in air. k is a skill factor: about 0.8 for a beginner, 0.3 for a modern factory using every trick.

Light Wavelength Smallest lines Era
Sun or mercury lamp, contact printing 350–450 nm 3–25 μm 1960s
Mercury lamp, projection 436 nm, 365 nm 1–0.35 μm 1975–1995
Krypton fluoride laser 248 nm 0.25–0.13 μm 1995–2003
Argon fluoride laser, lens dipped in water 193 nm about 0.04 μm 2006 on
Extreme ultraviolet from tin plasma 13.5 nm below 0.02 μm 2019 on

CMOS and the self-aligned gate

The simple chips of Integrated Circuits use one kind of transistor plus a resistor as its "load". Whenever an output is low, current flows through the resistor: a chip of a million such gates would melt. CMOS (complementary MOS) pairs each n-channel transistor with a p-channel one. One of the pair is always off, so no current flows except while switching. That is why chips can hold billions of transistors and run from a battery. It costs one extra step: a well, a deep island of opposite doping, for one kind of transistor.

In a metal-gate transistor the gate must overlap the source and drain to allow for misalignment, wasting space and speed. In 1968 Federico Faggin at Fairchild made the gate of polysilicon — silicon laid down from a gas as a film of tiny crystals — before the source and drain. The gate then shields the channel while dopant goes in on both sides, so everything lines up by itself. Nearly every chip since the mid-1970s is made this way.

Cut through two transistors and their wiring Not to scale. In a modern chip the whole drawing is about a quarter of a micrometre wide; in a 10 μm chip, about 100 μm. Passivation sealing layer Top metal thick, carries power Copper wiring 2 to 15 layers, joined by vias Metal 1 finest wiring Contact tungsten plug Trench glass between transistors Wafer p-type silicon Glass insulates every layer of wiring Gate on very thin oxide Source, drain heavily doped n-well for the p-channel transistor n-channel (nMOS) p-channel (pMOS)
Fig. 1 A modern CMOS chip in cross-section. The transistors lie at the bottom, in the silicon itself. Above them, layer on layer of copper wiring in glass connects them, fine at the bottom and thick at the top.

The silicon wafer

A wafer is a thin, round, mirror-polished slice of single-crystal silicon on which hundreds of chips are made at once.

Industrially, a crystal is pulled from melted Pure Silicon by the Czochralski method: a 300 mm crystal grows over two to three days to a cylinder up to 2 m long. It is ground to an exact diameter, and a small notch (or, on smaller wafers, a flat) is ground along one side to mark which way the atoms line up. A multi-wire saw — one steel wire about 0.12 mm thick and hundreds of kilometres long, wound over grooved rollers into hundreds of parallel strands and fed with diamond grit — cuts the whole crystal into slices in a few hours. The slices are edge-rounded, lapped flat, etched to remove saw damage, and polished on a cloth pad flooded with very fine silica in a weak alkali, which both rubs and dissolves the surface (chemical–mechanical polishing, CMP).

1 Crystal ground round; a flat marks its direction 2 Wire saw wires running in abrasive slurry 3 Slices 0.3–0.8 mm thick 4 Lap and polish on a turning pad with fine wet powder seed slurry Wafer 50–300 mm Flat crystal direction Chip hundreds per wafer Bond pads 0.1 mm square Circuit transistors and wiring Scribe lane for the saw Alignment mark Test structures in the lane
Fig. 2 From crystal to wafer. The crystal is ground round and marked with a flat, sliced by a wire running in abrasive, lapped and polished to a mirror. A finished wafer carries a grid of identical chips, separated by narrow lanes for the saw that also hold test structures.
Diameter Thickness In use from
25 mm about 0.25 mm 1960
50 mm 0.28 mm about 1969
100 mm 0.53 mm about 1975
200 mm 0.73 mm about 1992
300 mm 0.78 mm 2001

In the workshop: grow crystals 25–50 mm across, grind them round on a lathe with a silicon-carbide wheel (Abrasives and Grinding Stones), and grind a flat. Slice with a steel wire 0.2–0.3 mm thick running back and forth in silicon-carbide grit and oil; expect several hours per slice and to lose as much silicon as you keep. Lap each slice on glass with finer and finer grit, etch off 20–30 μm in a mix of Nitric Acid and hydrofluoric acid, and polish on felt with the finest silica or cerium oxide powder, kept wet.

Good or bad: a good wafer is a perfect mirror. Under one bright lamp in a dark room, looked at slantwise, any haze or scratch glows. Laid under a flat glass plate it shows only a few wide, straight coloured bands. Its thickness, checked with a dial gauge at five points, varies by no more than a few micrometres.

The photomask

A photomask is a glass plate carrying the pattern of one layer in an opaque film; a chip needs one per layer.

  • First masks: photographic emulsion on glass, drawn large and photographed down twice (Integrated Circuits). They scratch quickly; keep a master and print working copies.
  • Chromium masks: evaporate chromium 0.1 μm thick onto polished glass in vacuum (The Vacuum Pump), coat with resist, print the emulsion master onto it, and etch the chromium. The industry uses a cerium-salt etch; dilute Hydrochloric Acid also works once the reaction is started by touching the chromium with a zinc or aluminium rod. Chromium masks last thousands of prints and give sharper edges. Chromium metal comes from chromite (Chromium and Its Compounds, Electroplating).
  • Industrial reticles are 152 mm squares of fused quartz, 6.35 mm thick, carrying a chromium pattern four times final size, written directly by a computer-steered laser or electron beam. A transparent film (pellicle) on a frame a few millimetres above the pattern keeps dust out of focus.

Good or bad: inspect every mask at 100× under a The Microscope against a light, for pinholes, specks and ragged edges; measure a few lines with an eyepiece scale. Every layer must carry identical alignment marks in identical places.

What you need for a 10-micrometre line

Beyond the equipment of Integrated Circuits:

Item Notes
Clean room and clean bench Built as below; the heart of the line
Spin coater 1,000–6,000 turns a minute, vacuum chuck, splash bowl
Mask aligner Split-field microscope; stage screws moving 1 μm per division
Mercury lamp Strong ultraviolet (Arc Lamps, Neon and Fluorescent Lights), condenser lens, shutter
Three furnaces Fused-quartz tubes, one each for oxidation, diffusion and annealing, never mixed
Vacuum evaporator For aluminium and chromium, 0.01 Pa or better
Pure water Distilled twice, then through ion-exchange resin
Chemicals Sulfuric, nitric, hydrochloric, phosphoric and hydrofluoric acids; ammonia; hydrogen peroxide
Probe station Microscope, stage, four fine tungsten needles on screw holders, meters (Measuring Electricity)

Where to find it

The minerals are those of Integrated Circuits and Pure Silicon: quartz, fluorite for hydrofluoric acid, borax and rock phosphate for dopants, chromite for chromium. Gold for bonding wire comes from Gold and Silver, drawn to 25 μm through sapphire or diamond dies (Iron and Brass Wire, Synthetic Gems).

Hydrogen peroxide is made dilute as described in Hydrogen Peroxide and Oxygen Bleach. The cleaning baths below are written for peroxide of about 30 %, the strongest this book uses; with weaker peroxide, replace some of the water with extra peroxide so the bath holds the same amount. Never try to concentrate it. Ion-exchange resin is sulfonated polystyrene beads (Petrochemicals and Modern Plastics); until you have it, distil a third time in a quartz still.

Step by step: building the line

1. The clean room and clean bench

Clean Rooms covers the building in full; here is the minimum for a small line. Outdoor air holds tens of millions of particles larger than 0.5 μm per cubic metre, and a walking person sheds millions a minute. One particle on a mask or wafer kills the chip under it.

  1. The room: smooth painted walls, washable floor, sealed windows, fed with filtered air at slightly more than outside pressure so air always leaks out. Enter through a changing room. Wear lint-free gowns, caps, overshoes and gloves. No wood, paper, chalk or cotton wool inside. Wash the floor daily.
  2. The clean bench: a box about 120 cm wide, 60 cm deep and 70 cm high, open at the front. Its back wall is a filter: pleated paper of the finest Glass Fibre and Glass Wool you can draw (fibres 0.5–2 μm thick) in a frame sealed at every edge with wax. A fan in a closed box behind pushes air through it so that it flows evenly across the bench and out of the front at about 0.45 m/s — enough to make a thread held at the front stream steadily outward. A good filter of this kind ("HEPA") stops 99.97% of particles 0.3 μm across.
  3. Work only inside the bench, hands always downstream of the wafer.

Test: in a dark room, shine a narrow beam of light across the bench. In ordinary air you see dancing specks; in front of a good filter, almost none.

2. The spin coater

Mount a flat aluminium disc, smaller than the wafer, on the hollow shaft of a small The Electric Motor whose speed you can set. A 2 mm hole through disc and shaft leads to a vacuum line that holds the wafer flat. A bowl around it catches flying resist. Film thickness halves when speed is multiplied by four; for a 1 μm film of typical resist, about 3,000 turns a minute for 30 seconds. A good coat is evenly coloured, with no streaks running outward (dust) and no thick bead at the rim.

3. The mask aligner

  1. A heavy base of cast iron or stone on rubber feet, away from traffic.
  2. A wafer stage moving in X and Y and turning slightly on fine screws (Screws, Nuts and Bolts, Scientific Instrument Making). A 0.5 mm-pitch screw with a 100-division head moves 5 μm per division; a 10-to-1 lever makes it 0.5 μm.
  3. A mask holder above, and a way to lift the wafer into firm, even contact with the mask.
  4. A microscope with two objectives set a chip-width apart, so left and right alignment marks are seen side by side, lit by yellow light that does not expose the resist.
  5. A mercury lamp that swings in after alignment, with a timed shutter.

Always make the last move of each screw in the same direction, to take up backlash. With practice you will align to 1–2 μm, which is what a 10 μm process needs.

4. Clean every wafer the same way, every time

  1. Organic dirt: 10 minutes at 75–80 °C in 1 part ammonia solution, 1 part hydrogen peroxide (about 30%), 5 parts pure water.
  2. Metals: 10 minutes at 75–80 °C in 1 part hydrochloric acid, 1 part peroxide, 6 parts water.
  3. Thin oxide, when bare silicon is needed: a few seconds in 1 part hydrofluoric acid to 50 of water.
  4. Rinse in running pure water after each bath and dry with filtered air or nitrogen.

Test the water with two platinum wires 1 cm apart and a meter: tap water reads a few kilohms, good distilled water about a megohm, the best ion-exchanged water over ten megohms.

5. A 10-micrometre process

Start with the four-mask metal-gate process of Integrated Circuits, drawn at 10 μm. When it gives good transistors, improve it one change at a time:

  • Better resist. A positive resist — phenol–formaldehyde resin (Methanol and Formaldehyde, Coal Tar Chemicals) with a light-sensitive "diazo" compound — dissolves in weak alkali only where light fell, and does not swell, so it keeps fine edges. Making the diazo compound needs a skilled organic chemist; until then, gelatin resist will do.
  • Spin-on dopant. React silicon tetrachloride with dry alcohol to make a liquid that sets to glass; dissolve boric acid (p-type) or phosphoric acid (n-type) in it; spin it on, bake, and drive in at 1,000–1,100 °C. Cleaner and more even than powder sources.
  • n-channel transistors. Electrons move about three times faster than holes, so NMOS is faster, but far more sensitive to sodium. Switch once your gate oxide is clean.
  • Polysilicon gates, deposited at about 620 °C at low pressure from silane gas. See Dangers; many small lines stay with metal gates for years.
  • CMOS: one extra mask and a long well drive-in, several hours at 1,150 °C.

A 10 μm silicon-gate process uses five to seven masks. A 5 mm square chip then holds 2,000–5,000 transistors.

6. The chip package

Seen from above, lid off From the side legs fit holes 2.54 mm apart Leg 1 Notch Leg Chip glued down Gold wires 25 μm thick Lead frame thin metal sheet Body ceramic or epoxy 2.54 mm From the end 7.62 mm or 15.24 mm lid sealed over the chip
Fig. 3 A dual in-line package, opened up. The chip sits in the middle; gold wires thinner than a hair join its pads to the lead frame, whose legs come out through the sides.
  1. Probe every chip on the wafer; ink the bad ones.
  2. Separate the chips: industry uses a spinning diamond blade 20–50 μm thick, cooled with water; a diamond scribe and a gentle bend work on small wafers.
  3. Mount each good chip on a ceramic base or a lead frame stamped from thin copper or iron–nickel sheet (Sheet Metal and Rolling), with gold–silicon solder or silver-filled glue.
  4. Wire bond: join each pad (at least 0.1 mm square) to its lead with gold wire 25 μm thick, pressed on with a heated wedge at about 300 °C so gold and aluminium weld. Machines add ultrasonic vibration and make 10–20 bonds a second; by hand, under a microscope, a skilled worker makes a few hundred a day.
  5. Seal with a ceramic lid soldered on (best) or a moulded block of epoxy.

The dual in-line package (DIP) has legs 2.54 mm apart, in two rows 7.62 mm apart (up to 24 legs) or 15.24 mm apart (24–64 legs), and fits hand-made circuit boards and sockets.

How it is done in a modern factory

  • Wafers never meet air. They travel in sealed pods between machines on robot trolleys in the ceiling, through rooms thousands of times cleaner than outdoor air.
  • Layers are deposited from gases, sometimes one atomic layer at a time, or sputtered: knocked off a metal target by ions in a low-pressure glow.
  • Dopants are shot in by ion implantation: a small particle accelerator charges the dopant atoms, sorts them by weight with a magnet, speeds them through thousands to millions of volts and sweeps the beam over the wafer. A flash of heat lasting seconds then heals the silicon.
  • Etching is by plasma: a chlorine or fluorine gas, made to glow by radio waves at low pressure, attacks the surface while an electric field drives ions straight down, so walls stay vertical. Wet acid eats sideways too and cannot make lines much narrower than the film is thick.
  • Scanners project a quarter-size image of the reticle through a lens of 20–30 elements of fused quartz and calcium fluoride, while reticle and wafer slide in opposite directions, kept in step to a few nanometres. The newest use extreme ultraviolet made by hitting droplets of molten tin, 50,000 a second, with a powerful laser; nothing transmits such light, so the whole path is mirrors coated with dozens of alternating layers of molybdenum and silicon, in vacuum. One machine costs over 150 million dollars.
  • Wiring is copper, 10–15 layers. Trenches are etched in glass, lined with a barrier metal, filled by Electroplating, and polished flat by CMP before the next layer.
  • Transistors stand up: the channel is a thin fin or a stack of sheets wrapped by the gate on three or four sides. Names like "3 nm" are labels now; the smallest real repeated spacings are about 20–50 nm.

How to tell it worked

Every wafer carries test structures in the lanes between chips, measured first:

  • Sheet resistance of each doped layer, from four probes in a line, recorded every batch.
  • Contact chains: hundreds of contacts in series; one bad contact opens the chain.
  • Test transistors: the gate voltage at which each turns on (the threshold) should match from batch to batch within a tenth of a volt.
  • Ring oscillators: their frequency gives gate speed.

Yield, the fraction of chips that work, is the true measure of a line. With defects scattered at random:

yield ≈ e^(−D × A)

where D is killer defects per cm², A the chip area in cm², and e ≈ 2.72. With 1 defect per cm², a 1 cm² chip yields 37%; a 0.1 cm² chip, 90%. So a young line must make small chips. Map where the bad chips lie on every wafer and hunt the cause of every cluster.

Note Troubleshooting. Yield drops suddenly on every wafer → a dirty chemical, a leaking filter or a contaminated furnace; change one thing at a time and run test wafers. Bad chips at the edge → uneven resist, or furnace cooler at the ends of the boat. Bad chips in a line or ring → a scratch or particle on the mask; inspect and clean it. Thresholds drift → sodium, or gate oxide thickness varying; check the furnace and gases. Lines too wide or narrow → exposure or developing time wrong; print a test pattern of many widths. Layers shifted the same way across the wafer → backlash in the aligner.

Dangers

Danger Hydrofluoric acid is used in almost every step. It passes painlessly through skin and destroys bone and heart. Follow every warning in Integrated Circuits, and never work with it alone. Have calcium gluconate gel open beside you: after any splash, wash under running water for about 5 minutes, then rub in the gel at once and get medical help (Fluorspar and Fluorine Compounds).

Danger Silane catches fire by itself in air and can explode. Phosphine and arsine, which factories use as dopant gases, kill in a few breaths. A small line should use solid and spin-on dopants and avoid these gases. If you use silane, keep the cylinder outdoors in a vented steel cabinet, purge every line with nitrogen before and after, and burn the exhaust.

Danger Peroxide with sulfuric acid ("piranha") boils violently and explodes with solvents. Mix small amounts fresh and never close the vessel.

  • Ultraviolet lamps burn eyes and skin in seconds; shield them and wear glass spectacles.
  • Ion implanters use high voltage and give off X-rays; shield them in lead (X-Rays).
  • Waste acids and fluorides poison water. Neutralise with Lime, which turns fluoride back into harmless fluorite. Never pour into a stream.

The realistic road

Stage Lines Transistors per chip What it takes What you can make
1 25 μm, metal gate Tens to hundreds Integrated Circuits; a few dozen people Gates, counters, small memories
2 10 μm, silicon gate, chromium masks 2,000–10,000 A clean room, pure chemicals, spin-on dopants 8-bit Microprocessors and Personal Computers, 1–4 kilobit memories, calculator chips
3 3–5 μm, projection printing, plasma etch, ion implantation 30,000–150,000 Precision optics, accelerators, radio-frequency plasma 16-bit processors, 64-kilobit memories
4 1 μm, steppers, CMOS, two metal layers Up to a million An optics and chemical industry; hundreds of engineers Personal computers, digital radios, the first Flat Screens: LCD and LED Displays
5 0.25–0.13 μm, deep-UV lasers, copper, CMP 10–100 million A national industry Early mobile phones, internet routers
6 Below 0.05 μm, immersion and extreme UV Billions Many nations working together Smartphones, modern computers

Each stage took the world five to ten years, with the one before already running. Stage 2 is the 1970s: pocket calculators, digital watches, home computers and programmable controllers — enough to change everything.

What this unlocks

How it was first done

The first planar chips (1960) were made by hand on 25 mm wafers, with masks cut from red plastic film and photographed down. Gordon Moore predicted in 1965 that transistors per chip would keep doubling, and the industry made it true for fifty years. Faggin's silicon gate (1968) went into Intel's 4004 microprocessor of 1971, made with 10 μm lines on 50 mm wafers. Werner Kern devised the standard wafer clean at RCA in 1965. Perkin-Elmer's projection aligner (1973) ended the mask damage of contact printing; GCA sold the first wafer stepper in 1978. Ion implantation, patented by William Shockley in 1954, entered production in the 1970s; excimer-laser lithography was shown at IBM in 1982; IBM brought polishing and copper wiring (1997) into factories. Immersion lithography arrived around 2006, fin transistors in 2011, and extreme ultraviolet in volume production in 2019, after twenty years of development. At the other end of the scale, between 2018 and 2021 a student, Sam Zeloof, made working chips with hundreds of transistors in his parents' garage with second-hand equipment: the first rungs of the ladder are within reach of very few people.