◆ Rebuild

Part 2 · Earth and Fire

Very-High-Temperature Furnaces

How to get past the limits of fuel kilns and nichrome wire to 1,600–2,000 °C and beyond — oxygen-fed flames and the lime-block furnace, carbon resistance furnaces, silicon carbide and molybdenum disilicide heating elements, induction heating through a graphite susceptor — what to line them with, and how to measure heat so bright it hurts to look at.

Difficulty
●●●●●
Time
A day to build a lime-block furnace once you have oxygen; a week for a carbon tube furnace; months to make silicon carbide or molybdenum disilicide elements that last
Steps from zero
31 prerequisites →

You need first

Electric Kilns and FurnacesFirebrick and Refractories

This unlocks

—
The full path from nothing — 31 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Salt
  13. Bricks
  14. Fermentation
  15. The Wheel and Axle
  16. Firebrick and Refractories
  17. Bellows
  18. Gears
  19. Copper Smelting
  20. Iron (the Bloomery)
  21. The Waterwheel
  22. Blacksmithing
  23. Magnets
  24. The Battery
  25. Copper Wire
  26. Electrolysis
  27. Nickel and Cobalt
  28. The Generator
  29. Wiring and Electrical Safety
  30. Electric Kettles, Irons, Heaters and Cookers
  31. Electric Kilns and Furnaces
  32. Very-High-Temperature Furnaces

Do them roughly in this order. See it on the tech tree →

Why it matters

A good fuel kiln or wire-wound electric furnace stops at about 1,300–1,400 °C (The Kiln, Electric Kilns and Furnaces). Melting platinum (1,768 °C) and small steel melts (1,550–1,650 °C), firing alumina, magnesia and zirconia ceramics (1,600–1,750 °C, Firebrick and Refractories, Zircon and Zirconium), fusing quartz (1,800–2,000 °C, Fused Quartz and Halogen Lamps), sintering tungsten and carbides (Tungsten and Filament Wire), growing crystals and testing new firebrick all need more. Each hundred degrees above 1,400 °C is hard won. Here are four ways, simplest first.

How it works

Heat escapes faster the hotter you go. Radiated heat rises with the fourth power of absolute temperature (°C plus 273): going from 1,200 °C to 1,700 °C multiplies the loss by about 3.2. So very hot furnaces are small, heavily insulated and fed with concentrated heat.

Why ordinary flames stop. Fuel burned in air must also heat four volumes of nitrogen for each of oxygen, so a flame in cold air tops out near 1,900–2,000 °C in theory and far less in practice. Three ways past it:

  1. Preheat the air with the waste heat (the regenerators of the open-hearth furnace, Steel in Quantity).
  2. Use oxygen instead of air: methane, propane or hydrogen burned in pure oxygen gives 2,700–2,800 °C; acetylene and oxygen about 3,100 °C (Calcium Carbide and Acetylene).
  3. Use electricity, which has no flame temperature at all: the limit is only what the heater and the walls survive.

Every heater has a ceiling. The heater runs hotter than the work, so its own limit sets the furnace's:

Heater Element limit Furnace limit Atmosphere
Nichrome wire 1,200 °C 1,100 °C Air
Iron–chromium–aluminium wire 1,400 °C 1,300 °C Air
Silicon carbide rods 1,600–1,650 °C 1,500–1,550 °C Air
Molybdenum disilicide 1,800–1,850 °C 1,700 °C Air
Platinum–rhodium wire 1,700 °C 1,600 °C Air (very costly)
Molybdenum wire 2,000 °C 1,800 °C Hydrogen only
Graphite or carbon 3,000 °C 2,500 °C+ No oxygen: carbon monoxide, argon or vacuum
Electric arc 3,500 °C+ Beyond any wall Any (The Electric Arc Furnace)

Refractory choices

At these heats the walls fail before anything else. Choose the hot face for at least 100–150 °C above the working temperature, and back it with insulation that is good at its own temperature.

Material Melts at Safe working Notes
Fireclay 1,650–1,750 °C 1,400–1,500 °C Sags under load above this (Firebrick and Refractories)
Silica brick 1,710 °C 1,600–1,650 °C Rigid nearly to melting; cracks if cooled fast below 600 °C
Mullite / high alumina 1,810–1,850 °C 1,650–1,700 °C From bauxite or kaolin with alumina (Alum and Alumina)
Pure alumina 2,050 °C 1,800–1,850 °C Best all-round tube and crucible
Magnesia 2,800 °C 1,800–2,000 °C Resists basic slag; cracks with sudden heat; spoils in damp air
Stabilised zirconia 2,700 °C 2,000–2,200 °C Expensive; crucibles for platinum (Zircon and Zirconium)
Lime 2,570 °C 2,000 °C+ Very cheap; crumbles in moist air
Graphite none (vaporises 3,600 °C) 2,500 °C+ Only where there is no oxygen

Insulation behind the hot face: bubble alumina (hollow spheres made by blowing air through a stream of molten alumina from an arc furnace), light alumina brick, or, in carbon furnaces, loose lampblack or charcoal powder (Lampblack and Carbon Black), which insulates superbly where no air can reach it.

Neighbours must agree. Silica and alumina with a little lime, soda or iron melt where they touch, far below either's own melting point. Carbon eats oxides: it attacks silica above about 1,500 °C and magnesia above roughly 1,800 °C. Separate carbon from oxide walls with alumina or zirconia sand.

Heat and cool slowly, no faster than 100–200 °C an hour for thick dense walls; magnesia and silica crack most easily.

Method 1: The oxy-fuel and lime-block furnace

The burner

You need oxygen from liquid air (Liquid Air, Nitrogen and the Noble Gases) or from water split by electricity (Hydrogen, Oxygen and Gases), in cylinders or a gas holder, and a fuel gas: town gas, natural gas (Natural Gas and Helium), propane, or hydrogen.

Use a nozzle-mix burner: the gases travel in separate tubes and meet only at the tip, so a flame cannot run back into a pipe of ready-mixed gas.

  1. Inner tube: copper or brass, 4–8 mm bore, for oxygen; outer tube round it for fuel, the inner tip set back 1–2 mm. Above about 15 kW, water-cool the nozzle with a coil of copper tube.
  2. Safety: a non-return valve and a water-bottle flashback arrestor on each line, needle valves and pressure gauges (Pressure and Vacuum Gauges).

Mixing ratios by volume: hydrogen 2 : oxygen 1; methane 1 : 2; propane 1 : 5. Run slightly fuel-rich if the work must not oxidise, slightly oxygen-rich for a hotter, sharper flame.

Consumption: a 10 kW methane–oxygen burner uses about 1 m³ of methane and 2 m³ of oxygen an hour.

Oxygen enrichment, the easy step: add oxygen to the air of an ordinary gas or oil burner until it is 25–35% oxygen. The flame gets 200–400 °C hotter and the flue gas is smaller. This alone lifts a good kiln to 1,550–1,650 °C.

The lime-block furnace: the simplest version

This is how platinum was first melted in quantity (Platinum and the Platinum Metals). Quicklime (Lime) melts at about 2,570 °C, insulates very well, and soaks up impurities from the melt.

  1. Burn hard, pure limestone thoroughly and saw two sound blocks of quicklime about 15–20 cm across. Use them the same day: quicklime crumbles in moist air.
  2. Carve a hollow 4–6 cm across and 2–3 cm deep in the lower block, with a pouring lip. Hollow the upper block to match and bore a 15 mm hole down through it for the burner, plus a small side notch for gas to escape.
  3. Bind the blocks with iron wire on a firebrick, load the metal, and fire the oxy-hydrogen or oxy-gas burner down the hole. The inside glows brilliant white, like limelight.
  4. 100–500 g of platinum grains melt in 10–30 minutes. Tilt the whole block to pour into a lime or graphite mould.

Good versus bad. A good melt is a bright, mirror-smooth button. A dull or spongy one means too little heat: open the oxygen a little. A lime block glazed with a green or brown skin has picked up iron or copper from the charge — which is exactly what it is for.

The oxy-fuel box furnace

For bigger, steadier work, line a small box or cylinder with alumina or zirconia brick, 50–75 mm hot face, backed by 100–150 mm of bubble alumina and insulating brick, inside a steel case. Inside, a chamber of 10–15 cm each way. Fire one burner tangentially (aimed along the wall, not at the work) so the flame swirls round. Oxygen firing makes only about a fifth as much flue gas as air firing, so a flue hole 3–4 cm across is enough. It reaches 1,700–1,800 °C. Such furnaces test refractories, melt glass and metals in alumina crucibles, and fire small batches of special ceramics.

Method 2: Carbon resistance furnaces

Carbon carries electric current, never melts, and gets stronger as it gets hotter — as long as no air reaches it. That makes it the easiest way to reach 2,000 °C with electricity.

The granular carbon furnace

  1. Build a trough of firebrick about 50 cm long, 20 cm wide and 20 cm deep, with a carbon electrode (a block of arc-furnace electrode, The Electric Arc Furnace) let into each end.
  2. Fill it with granular carbon: crushed coke or graphite, 2–5 mm grains, sieved free of dust (Ball Mills, Crushers and Grinders).
  3. Bed a crucible of graphite, alumina or magnesia in the middle of the carbon, and cover everything with a 5 cm blanket of dry sand.
  4. Pass current from one electrode to the other through the granules: 50–100 volts from a transformer with taps (The Transformer), at a few kilowatts. Current flows through the countless small contacts between grains, and each contact glows. Pack the grains more tightly, or put the electrodes closer, for more current.

It reaches 1,700–2,000 °C round the crucible. Top up the coke as the surface burns away.

The carbon tube furnace

Thin middle: white-hotup to 2,000–2,500 °C Graphite tube Lampblack packinginsulates, keeps air out Copper clampwater-cooled Work in a boat Steel box transformer: 8–20 V, 500–1,500 A pyrometer gas burnt argon water
Fig. 1 The carbon tube furnace in section. A graphite tube is clamped between two water-cooled copper blocks fed by a heavy low-voltage transformer. Current heats the tube white-hot along its thin middle. It sits in a steel case packed with lampblack or charcoal powder, which insulates it and keeps air away. The work sits in a boat in the hottest part; an optical pyrometer sights along the bore, and gas flowing through the tube is burnt where it comes out.

The carbon tube furnace makes a clean, even hot zone that you can look into.

  1. The tube: turn a graphite tube from an arc-furnace electrode on the lathe (The Lathe): 2.5–4 cm bore, 30–40 cm long, the wall 3–5 mm thick over the middle 15–20 cm and thicker at the ends, so the middle has more resistance and gets hottest.
  2. The clamps: two thick copper blocks bored to grip the tube ends, each with a water channel through it or a copper water pipe soldered on (Soldering and Brazing). Without water they melt.
  3. The power: a step-down transformer giving 8–20 volts at 500–1,500 amps — the same kind of transformer as an arc welder (Welding), with taps or a choke to adjust it. A tube of these sizes takes 5–15 kW for 2,000 °C.
  4. The packing: stand the tube in a sheet-steel box filled with lampblack or fine charcoal powder 10–15 cm deep all round. It keeps air from the tube and keeps the heat in.
  5. Sighting: look along the bore from one end with an optical pyrometer to read the work's heat.
  6. Gas: blow a gentle stream of nitrogen or argon (Liquid Air, Nitrogen and the Noble Gases) through the tube, or simply let the carbon make its own carbon monoxide; burn the gas at the outlet.

Raise the power in steps over 30–60 minutes. A good tube runs for dozens of firings; it fails by burning thin at a spot where air leaks in. The inside is strongly reducing (it takes oxygen out of things), which suits melting metals, sintering carbides and making metals from oxides, but turns many oxide crucibles to carbide or metal: line the work boat with zirconia or alumina powder, and test first.

Method 3: Silicon carbide and molybdenum disilicide elements

To go above 1,300 °C in air with electricity, you need a heater that does not burn. Two materials do this by growing a thin skin of silica glass that seals the surface.

Silicon carbide rods, furnace front section Hot zonethin, glowing Cold endthick, low resistance Terminalaluminium-sprayed, braid work alumina hot facebubble aluminainsulating bricksteel case Molybdenum disilicide Thick legsthrough roof Hairpinto 1,850 °C hangs free
Fig. 2 Left: a silicon carbide rod element in a furnace wall. The thin hot zone runs across the chamber; the thick cold ends pass through the walls to aluminium-sprayed terminals and braid outside. Right: a molybdenum disilicide hairpin hanging from the roof, with thick terminal legs. Below: the furnace wall in layers — alumina hot face, bubble alumina, insulating brick, steel case.

The silicon carbide element

What it is. A rod of silicon carbide (carborundum), 8–50 mm across and 30 cm to 2 m long. The middle, the hot zone, is thinner or more porous and has high resistance; the two ends, the cold ends, have low resistance so they stay cool where they pass through the walls. The furnace reaches 1,500–1,550 °C in air, and the rods last 2,000–5,000 hours.

Making one. Silicon carbide grain comes from the carborundum furnace (Precision Grinding, Abrasives and Grinding Stones). The rod must be bonded by silicon carbide itself, because no clay survives.

  1. Grain: mix about equal parts of coarse (0.3–1 mm) and fine (under 0.05 mm) silicon carbide, with 10–15% fine carbon (lampblack or ground petroleum coke) and 10–15% silicon powder (Pure Silicon gives the method), plus a temporary binder of dextrin or tar.
  2. Shape: extrude or press rods, then dry them.
  3. Fire in a carbon tube or granular carbon furnace, packed in carbon, at 1,500–1,700 °C for several hours. The silicon melts, soaks into the rod and reacts with the carbon to form new silicon carbide that welds the grains together. The early German elements of the 1900s were made in a similar way.
  4. Cold ends: make them thicker, or soak them in molten silicon, so their resistance is a fifth or less of the hot zone's.
  5. Terminals: spray or melt aluminium onto the last 3–5 cm, and clamp flexible aluminium or copper braid onto it.

Using it. Load the hot zone lightly when the furnace runs hot: up to about 10 W per cm² of rod surface for a furnace at 1,300 °C, but only 3–5 W per cm² at 1,450–1,550 °C. A 12 mm rod with a 30 cm hot zone (about 110 cm² of surface) therefore takes roughly 0.4–0.6 kW at top heat.

  • Ageing. Resistance falls as a rod warms to about 800 °C, then rises. Over its life the silica skin thickens and resistance creeps up two or three times. Feed rods from a transformer with several voltage taps, start on the lowest, and step up over the months. Group rods of equal resistance in series.
  • Mounting: horizontally through holes in the side walls, at least two diameters apart and from floor and roof, free to expand.
  • Enemies: hydrogen, steam and alkali vapours from glazes, salt or a damp new lining.

The molybdenum disilicide element

What it is. A hairpin or U of molybdenum disilicide (a compound of molybdenum and silicon), 3–12 mm thick, hanging from the furnace roof, with thicker legs as terminals. It runs at up to 1,800–1,850 °C itself, so the furnace reaches 1,700 °C in air — the highest of any air-going element.

Its odd habits:

  • Very low resistance that rises about ten times from cold to hot. It needs a heavy low-voltage transformer (tens of volts) with a current limiter or a slow start; cold, it draws a huge surge.
  • Brittle when cold, soft when hot (above about 1,200 °C), so it must hang, never lie on a support, and it will bend under its own weight if mounted sideways.
  • "Pest": held for long at 400–700 °C it can crumble to powder, because the protective glass cannot form at that heat. Pass through that range quickly, both up and down.

Making one, in outline: roast molybdenite to oxide and reduce it in hydrogen to molybdenum powder (Molybdenum), much as for Tungsten and Filament Wire. Heat it with silicon powder in argon; it reacts to molybdenum disilicide. Grind that (Ball Mills, Crushers and Grinders), mix with 10–20% fine clay, extrude rods, sinter at about 1,500–1,600 °C in hydrogen, bend hot, and weld on thicker legs. Expect many failures; use silicon carbide first.

Good versus bad, for both: a good element glows evenly along its hot zone. A brighter spot is a thin or cracked place that will burn through; a dull end means a poor terminal contact — clean and re-clamp it.

Method 4: Induction with a graphite susceptor

Coilwater-cooled copper tube,10–400 kHz Insulationcarbon felt or lampblack Quartz tubethe field passes through Graphite susceptorinduced current heats it;wall 1½ skin depths Crucible and meltheated by radiation Argon fillstops graphite burning optical pyrometer argon in out
Fig. 3 Induction heating with a graphite susceptor. A water-cooled copper coil surrounds a quartz or alumina tube. Inside, a graphite cylinder — the susceptor — picks up the induction currents and glows white; it radiates its heat into a crucible of glass, quartz or ceramic, which the coil alone could not heat. Carbon felt or lampblack insulates it, and argon keeps the graphite from burning.

An induction coil heats only things that conduct electricity (Electric Kilns and Furnaces). Glass, quartz, oxides and small metal charges barely warm. The answer is a susceptor: a piece of graphite inside the coil that the field heats, and that then radiates heat into the work.

Sizing the susceptor. Induced current flows in a skin near the surface. In graphite the skin depth is much larger than in metal, because graphite conducts poorly:

Frequency Skin depth in hot graphite Susceptor wall
3,000 Hz about 3 cm 4–6 cm (big susceptors only)
10,000 Hz about 1.6 cm 2.5–3 cm
100,000 Hz about 5 mm 8–10 mm
400,000 Hz about 2.5 mm 4–5 mm

Make the wall at least 1½ times the skin depth so it takes up nearly all the power; a wall much thinner lets the field through to heat nothing.

Building it.

  1. Susceptor: turn a graphite cup or tube from electrode stock (The Electric Arc Furnace), with a lid that has a sight hole.
  2. Insulation: surround it with 2–4 cm of lampblack, carbon felt, or zirconia or alumina bubble, held in a tube of fused quartz or alumina (Fused Quartz and Halogen Lamps). Quartz lets the field through and does not heat.
  3. Coil: 6–12 turns of water-cooled copper tube round the outside of the quartz tube, from a valve oscillator or motor-alternator (Amplifiers and Oscillators, The Generator).
  4. Atmosphere: graphite burns in air above about 500 °C and quickly above 700 °C. Flush the tube with argon or nitrogen, or pump it to a vacuum (The Vacuum Pump).

A susceptor of 5 cm across in a 10–20 kW, 10,000–400,000 Hz supply reaches 2,000–2,500 °C. It melts glass and quartz, grows crystals in quartz crucibles (Pure Silicon), and heats in vacuum with no flame or element in the way.

Measuring the heat

Thermocouples of platinum against platinum–rhodium reach 1,450–1,500 °C (Pyrometric Cones and Kiln Temperature). A pair of two platinum–rhodium alloys (30% and 6% rhodium) reaches about 1,700–1,800 °C. In carbon or inert furnaces, tungsten against tungsten–rhenium reaches 2,300 °C, but burns instantly in air.

The optical pyrometer (Pyrometric Cones and Kiln Temperature) is the main tool above 1,500 °C. With a calibrated smoked-glass filter in front of the lamp it reads to 2,000 °C and beyond. Sight into a hole or the far wall of the hot zone, which glows as a true blackbody; a bare white-hot surface in the open reads too low.

Check points. Hang short pieces of pure wire in the hot zone and see which melt: nickel 1,455 °C, iron 1,538 °C, palladium 1,555 °C, platinum 1,768 °C, rhodium 1,964 °C. High cones of kaolin with stepped additions of alumina bend between about 1,600 and 2,000 °C; calibrate your own series against the wires.

Your eyes see only dazzling white above 1,400 °C. Look through welding glass, shade 5–8 for furnaces (Welding).

How to tell it worked

  • The wire test: a platinum wire in the hot zone melts into a bead — you are above 1,768 °C.
  • The cone test: your high cone bends at the expected place, run after run.
  • Even heat: two test cones or wires at either end of the hot zone behave alike; elements glow evenly.
  • Clean walls: no glazing, dripping or bloating of the hot face after a firing.

Note Troubleshooting. Furnace stalls below its target → poor insulation (feel the case: if too hot to touch for a second, add insulation), too little power, or element tap set too low. Hot face drips or glazes → refractory too low-grade, or fluxed by vapours from the charge; use purer alumina or zirconia and keep salts and glazes out. Graphite tube burns through → air leaking in; repack the carbon powder and add an inert gas flow. Silicon carbide rods failing quickly → overloaded (too many watts per cm²), steam from a damp new lining, or alkali from the work. Disilicide element crumbled → it lingered at 400–700 °C; ramp through that range faster. Oxy-fuel flame pops back → gas too slow for the nozzle; raise the flow, clean the tip, and check the flashback arrestors.

Dangers

Danger Oxygen makes everything burn. Oil, grease, clothing and even steel burn fiercely in oxygen. Never oil an oxygen valve or regulator; keep oxygen lines clean and dedicated; never use oxygen to blow dust off clothes. Store fuel and oxygen apart, use flashback arrestors on both lines, and open the fuel first when lighting.

Danger Carbon furnaces make carbon monoxide, which kills without smell. Burn the gas at every outlet, work under a hood, and never lean over the box. Huge currents at low voltage do not shock, but they make severe burns where a ring, watch or tool closes the circuit: take off metal jewellery.

Danger Cooling water. If the water stops, a coil or clamp melts in a minute; if water then meets molten metal or white-hot carbon, it flashes to steam explosively. Fit a flow switch that cuts the power when the water stops, and keep all water lines away from where melts can spill.

  • Bright light and infrared burn the retina and cloud the eye's lens over years; always use dark glass.
  • Dust of silicon carbide, alumina, fibre and quartz scars the lungs: grind wet, wear a respirator.
  • Damp lime blocks can burst; quicklime burns wet skin and eyes (Lime).

What this unlocks

Melting Platinum and the Platinum Metals gives thermocouples, crucibles and the electrodes of electrochemistry. These furnaces make Fused Quartz and Halogen Lamps tubes and crucibles, alumina and zirconia ceramics, the sintered tungsten and carbides of Tungsten and Filament Wire and Powder Metallurgy, test bricks for Steel in Quantity and The Electric Arc Furnace linings, and grow crystals for Pure Silicon, Synthetic Gems and Lasers. They are the furnaces of Making Microchips.

How it was first done

In 1801 Robert Hare in Philadelphia built an oxyhydrogen blowpipe and melted platinum in small amounts. In 1857 Henri Sainte-Claire Deville and Jules Debray in Paris melted kilograms of platinum in blocks of lime heated by oxygen and coal gas, which made platinum a practical industrial metal. Henri Moissan in Paris used an electric arc inside lime blocks in 1892 to reach about 3,500 °C. Edward Acheson made silicon carbide in 1891 in Pennsylvania. Gustav Tammann in Göttingen built carbon tube furnaces in the early 1900s, and granular carbon furnaces were sold in Germany at about the same time. Silicon carbide heating rods appeared in Germany in the 1900s and in the United States in the 1920s. Edwin Northrup in Princeton developed high-frequency induction furnaces around 1916–1920, and molybdenum disilicide elements were introduced in Sweden in 1956.

Source: content/entries/earth/high-temperature-furnaces.md