Wire Rope and Cable

Twist iron or steel wires into strands and strands into rope, round a tarred hemp heart, and you get a rope six to ten times stronger than hemp of the same size that never rots. How to lay it on a ropewalk, choose its construction, keep it greased, end it with splices, clips and poured sockets, and inspect it so it never fails with a load — or a cage of miners — on the end.

Difficulty
●●●●●
Time
A day to set up a ropewalk for wire; a day to lay 50–100 m of small rope by hand; an hour to splice or socket an end
Steps from zero
22 prerequisites →

You need first

Iron and Brass WireRopewalks and Sailcloth

This unlocks

Lifts, Hoists and Mine Winding
The full path from nothing — 22 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Farming from Seed
  11. Spinning and Weaving Cloth
  12. Hides and Leather
  13. Flax, Hemp and Linen
  14. The Loom
  15. Bellows
  16. Ropewalks and Sailcloth
  17. Iron (the Bloomery)
  18. Copper Smelting
  19. Blacksmithing
  20. Steel
  21. Copper Wire
  22. Iron and Brass Wire
  23. Wire Rope and Cable

Do them roughly in this order. See it on the tech tree →

Why it matters

Hemp rope is strong for its weight, but it stretches, it rots when wet, and above a certain size it becomes too heavy to lift itself. Chains are strong but heavy, and they break without warning when a single link has a hidden flaw. Wire rope solves both problems. A steel wire rope as thick as your finger lifts as much as a hemp rope as thick as your wrist. It lasts for years in wet mines and on ships. And because it is made of hundreds of wires, it does not break all at once: wires snap one by one, where you can see them, long before the rope fails.

That made possible:

How it works

Cross-sections (enlarged) One strand1 + 6 wires 6×7, fibre corethick wires: stiff, resistswear and rust 6×19, fibre corefiner wires: the general-purpose crane and hoist rope Coretarred hemp,holds grease Side views Regular laywires run along the rope; holds its shape,resists kinks — the usual choice Lang's laywires run across the rope; wears longer,but untwists: fix both ends
Fig. 1 Wire rope construction. Wires are twisted into strands, and six strands into a rope round a core. In regular lay the wires run along the rope; in Lang's lay they run across it.

Wire rope is built exactly like fibre rope (Ropewalks and Sailcloth), one level higher:

  1. Wires are drawn from good iron or, much better, high-carbon steel (Iron and Brass Wire).
  2. Strands. The simplest strand has 7 wires: one straight centre wire with six wires of the same size twisted round it. Six circles fit perfectly around one of the same size, so the strand is round and tight. Bigger strands add a second layer: 1 + 6 + 12 = 19 wires.
  3. Rope. Six strands are laid round a core.

The core is the heart of the rope. A fibre core — hemp soaked in tar and grease — gives the strands a soft bed, keeps the rope round, and holds grease that slowly feeds the wires from inside. A wire core (a small 7-strand rope of its own) is stronger and does not crush on a drum, but is stiffer and harder to make.

Lay. In regular (ordinary) lay, the wires in each strand are twisted the opposite way to the strands in the rope, so the wires on the surface run roughly along the rope. Regular lay holds its shape, resists kinking and untwisting, and is the right choice for most work. In Lang's lay (Albert's lay), wires and strands twist the same way, so the surface wires run across the rope at an angle. More of each wire touches the sheave, so it wears longer and bends more easily — but it tends to untwist under load, so both ends must be fixed (never on a single free-hanging hook).

Construction names. A rope is named strands × wires: 6×7 (6 strands of 7 wires: few, thick wires; stiff, but survives rubbing and rust — haulage, guys, mine shafts on big drums), 6×19 (the general-purpose rope: cranes, hoists, winches), 6×37 (many fine wires; very flexible, for small sheaves, but wears faster).

Strength. Rope strength goes with the square of its diameter. For good hard-drawn steel wire rope of 6×19 construction:

Breaking load (tonnes) ≈ 0.055 × d², with d the rope diameter in mm.

So a 10 mm rope breaks at about 5.5 tonnes, a 20 mm rope at about 22 tonnes. Iron wire rope is roughly a third as strong; hemp rope of the same size, roughly a sixth to a tenth. Safe working load is the breaking load divided by a safety factor: 5 for cranes and general lifting, 8–10 for anything that carries people (mine cages, lifts), and more for a hand-made rope that has not been tested.

Bending. Every time a rope runs round a pulley (a sheave) or a drum, the wires bend and rub. Too small a sheave kills a rope fast. The sheave diameter (at the bottom of the groove) should be at least:

Construction Absolute minimum sheave or drum diameter Better, for long life
6×7 42 × rope diameter 70 ×
6×19 30–34 × rope diameter 45–50 ×
6×37 23 × rope diameter 35 ×

So a 12 mm 6×19 rope wants a sheave at least 36 cm across, and lasts far longer on one of 55–60 cm. The groove should be a smooth half-round just 5–10% wider than the rope.

What you need

Item Amount Notes
Wire About 1.1 × rope length × number of wires Steel wire, patented and hard-drawn, 1–3 mm; or soft iron for a first rope (Iron and Brass Wire). Galvanised for wet work (Zinc and Brass)
Hemp core One length of 3-strand hemp rope, the size of a strand Ropewalks and Sailcloth
Rope grease A bucket Pine tar and tallow, about 1 : 1, melted together (Tar, Pitch and Glue)
Ropewalk 10–20% longer than the rope As for hemp rope, with a stronger jack and sledge
Jack Iron hooks on cranked gears One hook for stranding; six for closing (Gears)
Lay plates Iron discs with holes One with a centre hole and 6 holes in a ring (strands); one with a centre hole and 6 notches (closing)
Seizing wire Soft annealed iron, 1 mm For binding ends before cutting
Marlinspike Tapered steel spike 25–40 cm For splicing
Leather gloves — Broken wire ends pierce hands

Step by step: laying a small rope by hand

This makes a 6×7 rope with a hemp core, about 8–12 mm thick, by the same method as a hemp rope.

  1. Prepare the wire. Draw it to size, anneal or patent it, and wipe it with grease. For a 10 mm rope, use wires of about 1.1 mm: each 7-wire strand is then about 3.3 mm, and six strands round a 3.3 mm core give a rope of about 10 mm.
  2. Lay out the strand wires. Stretch seven wires side by side down the ropewalk under light tension. At the jack end, clamp all seven together into one hook. At the far end, fasten them to a hook on a heavy sledge that is held from turning.
  3. Thread the lay plate. Near the sledge, pass the centre wire through the centre hole of the stranding plate and the six others through the ring of holes.
  4. Strand. Turn the jack. The six outer wires wrap round the centre wire just ahead of the plate. Walk the plate slowly toward the jack so that the twist is even: aim for one full turn of the outer wires in about 8 strand diameters (about 27 mm for a 3.3 mm strand). Count jack turns per metre and keep it constant. Make six strands this way, all with the same direction of twist.
  5. Preform (recommended). Before closing, wrap each strand once round a pipe or rod of about 4 times its diameter and pull it through: this sets a gentle helix so the finished rope lies quiet and its cut ends do not spring apart.
  6. Close the rope. Hook the six strands to the six hooks of the closing jack, run the greased hemp core down the middle, and bring everything together through the closing plate at the sledge end. Turn the jack hooks so each strand keeps its own twist (not unwinding), while the sledge hook turns the other way to lay the strands round the core. Walk the closing plate toward the jack. For regular lay, the strands must be twisted the opposite way to the wires. The finished rope should make one full turn of each strand in about 6.5–7.5 rope diameters.
  7. Grease as you lay. Paint hot rope grease into the strands just ahead of the closing plate.
  8. Seize the ends before you release them (below), then let the rope hang straight under a weight overnight.

Factory machines do the same job far faster with all the wire bobbins carried on a turning frame. The best machines (planetary stranders) keep each bobbin facing the same way as it goes round, so the wires are not twisted on their own axes. A hand-laid rope twists each wire a little; it is fine for light work but should be tested before use.

Ends and joins

Thimble eye with clipsPoured socket 6 rope diameters U-bolton the short dead end Dead endseized Live endcarries the load Saddle on the live end"never saddle a dead horse" Thimblegrooved ring Pin eye Zincpoured at480–540 °C Broomof cleanwires Seizing the cone of zinc and wires cannotpull through: full rope strength Discard the rope when you see 6 broken wires in one lay length birdcage: strands opened out kink: cut it out
Fig. 2 Ending a wire rope. A thimble eye held with clips: the U-bolts always go on the short dead end. A poured socket keeps the full strength of the rope.

Seizing. Before you cut a wire rope, bind it tightly on each side of the cut with soft iron wire, wound for a length of 1–2 rope diameters, so the strands cannot spring apart. Cut with a hardened chisel on an anvil, or a hacksaw (Files and Saws).

The thimble eye with clips. For a quick, strong eye:

  1. Bend the rope round a thimble — a grooved iron ring that protects the rope from crushing.
  2. Fit U-bolt clips (bulldog grips). The U-bolt goes on the short dead end; the saddle goes on the long live end that carries the load. ("Never saddle a dead horse.") A U-bolt on the live end crushes it.
  3. Use 3 clips for ropes up to 16 mm, 4 up to 22 mm and 5 for 25 mm, spaced 6 rope diameters apart. The first clip goes one saddle-width from the end; the last as close to the thimble as you can.
  4. Tighten evenly, apply the load, then tighten again. The rope thins under load and clips loosen. Check them often. A clipped eye holds about 80% of the rope's strength.

The spliced eye. Unlay the end for about 30–40 rope diameters, cut out the core, bend the rope round a thimble, and tuck each strand under the strands of the main rope with the marlinspike — each strand in turn, against the lay, at least five full tucks, pulling each one tight and hammering it down with a mallet over a block of wood. A good splice holds 80–90% of the rope's strength. It is harder than splicing hemp: practise on soft iron rope first, wear gloves, and fix the rope in a vice.

The poured socket — for mine hoists, bridges and anything critical. It holds the full strength of the rope.

  1. Slide a cast-steel socket (a short tube with a tapered bore, wider at the mouth that faces away from the rope) onto the rope.
  2. Seize the rope where the socket's narrow end will sit. Unlay the end above the seizing, cut out the fibre core, and spread all the wires into a broom the length of the socket's cone.
  3. Clean every wire bright: scrub off the grease with a solvent (Ether, Acetone and Solvents), dip in dilute Hydrochloric Acid for a minute, rinse, and dip in a zinc chloride flux (Soldering and Brazing).
  4. Pull the socket up over the broom until the wire ends are level with its mouth. Hold the rope straight and vertical, socket up, with clay packed round the bottom to seal it.
  5. Warm the socket until water sizzles on it, then pour molten zinc, well above its melting point but not glowing (about 510–540 °C; zinc that glows red is too hot and weakens the bond and the wires; see Zinc and Brass), to fill it in one pour. Let it cool slowly without moving it.

The wedge of zinc and wires cannot pull through the cone. A white-metal (lead–antimony–tin) filling is acceptable for light loads only.

Endless ropes for haulage are joined with a long splice, 600–1,000 rope diameters long in all: unlay both ends, and lay each strand of one rope into the gap left by the matching strand of the other, staggering the joints along the rope and tucking each end into the core. It keeps the rope's diameter unchanged so it runs over sheaves.

Use and care

  • Uncoiling. Never pull a wire rope off a coil lying still on the ground — it will twist and kink. Roll the coil along the ground like a wheel, or put it on a turntable or a shaft through its middle and draw the rope off straight.
  • Kinks. A loop pulled tight into a kink is permanent damage: the rope has lost much of its strength at that spot. Cut it out.
  • Drums. Wind the first layer tight and close. Keep the fleet angle — the angle between the rope and the drum's centre line as it travels across — under about 1.5°: at least 40 m from drum to first sheave for every metre of sideways travel.
  • Grease. Every few weeks in use, brush or drip a thin mixture of tallow, tar and a little oil onto the rope where it bends over a sheave, so it soaks in. A dry rope rusts from the inside, where you cannot see it.
  • No sharp edges. Pad any corner the rope is pulled over with wood or a split pipe.

How to tell it worked

  • Shape. A good rope is round, with strands evenly spaced and the same height all round. Roll it on a flat floor: it should roll smoothly without a lump in any one strand.
  • Lay length. Mark one strand with chalk; one full turn should take about 6.5–7.5 rope diameters, the same all along.
  • Proof test. Before first use, hang twice the working load on the rope (or on a sample from the same batch) for 10 minutes, over a soft landing, everyone clear. Nothing should slip, crack or pull out. For carrying people, break a sample length from every batch with a lever or a screw press and keep a record (Strength of Materials).

Inspection — weekly for working ropes, daily for mine winding ropes. Run the rope slowly while someone watches each part pass, and look and measure:

Sign Discard when
Broken wires 6 broken wires anywhere in one lay length, or 3 in one strand in one lay length, or any broken wire at a socket or clip
Wear Diameter, measured across the strand crowns with callipers, down by 5% or more from new; or outer wires worn flat to a third of their thickness
Kink, crush or flattening Any permanent kink; any flattened section
Birdcage Strands opened out like a cage — the rope has been suddenly unloaded or twisted
Core sticking out Any
Heat damage Blue or straw colours from fire, welding or lightning
Rust Pitted wires, or rust powder squeezing out from inside

Note Troubleshooting. Rope will not lie straight, writhes and twists when slack → strands or wires not preformed, or lay uneven. Preform the strands, and keep the turns per metre steady. Cut ends burst apart → no seizings, or rope not preformed. Always seize both sides before cutting. Wires break after a few weeks at one place → that is where the rope bends over a sheave that is too small or has a worn, too-narrow groove. Fit a bigger sheave, reshape the groove. Rusty inside, bright outside → dry fibre core. Grease more often, and soak cores well before laying. Clips slipping → clips on backwards, or not retightened after the first load. Rope untwists and spins the load → Lang's lay on a free hook. Use regular lay, or fix both ends.

Dangers

Danger Snap-back. A loaded wire rope stores huge energy. If it, its eye or its anchor fails, the ends whip back faster than you can move and can cut a person in half. Never stand in the bight (inside the angle of a rope round a sheave), in line with a rope under tension, or under a suspended load. Mark and keep clear of these zones when a rope is being tested or pulled hard.

Danger Carrying people. Mine cages and lifts need ropes with a safety factor of 8–10, poured sockets, daily inspection, regular renewal on a fixed schedule whether they look worn or not, and a separate safety catch that grips the guides if the rope breaks. A single weak rope will kill everyone in the cage.

  • Broken wires stick out like fish hooks and tear hands. Wear leather gloves and never slide a bare hand along a rope.
  • Drums and sheaves pull in hands and clothing. Never guide a moving rope by hand near a drum.
  • Hot zinc for sockets: everything must be dry. See Metal Casting.

What this unlocks

Deep shafts and winding engines for Mining and Tunnelling; heavy Cranes and Lifting and lifts for Steel Frames and Tall Buildings; aerial ropeways; cable-hauled inclines for Railways; suspension bridges (Roads and Bridges); masts and guy ropes for Radio and Wind Turbines towers; ship rigging (Boats and Sails, Steamships); armour for submarine The Telegraph cables.

How it was first done

The mining official Wilhelm Albert made the first practical wire ropes in the Harz mountains of Germany in 1834, for the shafts at Clausthal, where hemp ropes and chains kept failing. His ropes were laid by hand from iron wire, with the wires and strands twisted in the same direction — the style still called Albert lay or Lang's lay. Within a few years wire ropes were being made in Britain, notably by Andrew Smith in London and by Robert Newall, who patented a rope-making machine in 1840. In the United States, John A. Roebling began making wire rope in Pennsylvania in 1841 to haul canal boats over the Allegheny Portage Railroad, and went on to build suspension bridges. Elisha Otis demonstrated his safety lift in New York in 1854, Andrew Hallidie's cable cars started in San Francisco in 1873, and John Lang of Scotland patented his lay in 1879. The great cables of the Brooklyn Bridge (1883) were not stranded rope at all but thousands of parallel steel wires spun across the river one by one and bound together.