◆ Rebuild

Part 3 · Metals

The Electric Arc Furnace

An electric spark the size of your thumb, burning steadily between a carbon rod and the metal, is hotter than any fire. Built into a lined box, it melts steel scrap, and with the rod buried in the charge it makes ferroalloys, calcium carbide and silicon — things no fuel furnace can.

Difficulty
●●●●●
Time
Months to build the power plant and furnace; weeks to make and bake electrodes; 2–4 hours per melt
Steps from zero
23 prerequisites →

You need first

The GeneratorFirebrick and Refractories

This unlocks

Calcium Carbide and AcetyleneIndustrial Diamond and Hard AbrasivesPure SiliconAlloy and Stainless SteelsAluminiumTitaniumWelding
The full path from nothing — 23 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Bricks
  13. The Wheel and Axle
  14. Firebrick and Refractories
  15. Bellows
  16. Gears
  17. Iron (the Bloomery)
  18. Copper Smelting
  19. The Waterwheel
  20. Blacksmithing
  21. Magnets
  22. Copper Wire
  23. The Generator
  24. The Electric Arc Furnace

Do them roughly in this order. See it on the tech tree →

Why it matters

Every furnace in this book so far has been limited by its fuel. Charcoal and coke burning in air can just reach about 1,700 °C, and the hot gases they make — carbon monoxide, carbon dioxide, sulfur from coal — get into the metal. An electric arc is different. It is a continuous spark burning in a column of glowing gas at 3,000–6,000 °C. It needs no air, makes no ash, and puts its heat exactly where you aim it.

With an arc furnace you can:

It is also the reason to build big electric power. A furnace that does useful work needs tens of kilowatts — about a hundred times the dynamo in The Generator. Plan the furnace and the power plant together.

How it works

The arc

Bring two carbon rods carrying a current into contact, then draw them a little apart: the current keeps flowing through the air gap as a dazzling, roaring flame. This is the arc. The air in the gap has been heated until it conducts electricity, and the current passing through keeps it hot. Carbon is used for the rods because it does not melt — it turns to vapour only at about 3,600 °C — and it conducts well when hot.

In a direct arc furnace, the arc jumps from a carbon electrode (the rod) straight onto the metal, and the current passes through the metal itself. In a submerged arc furnace, the electrode is buried deep in a charge of ore and coke; the heat comes partly from small arcs and partly from current flowing through the hot charge, like the element of a stove.

Low voltage, high current

An arc a few centimetres long needs only 40–100 volts. All the heat comes from current: hundreds or thousands of amperes. Power is volts times amps: 50 V × 400 A = 20,000 W, or 20 kW. So the arc furnace needs a special supply — not high voltage, but heavy current at low voltage, carried by thick copper or iron bars.

The arc must be tamed

An arc has a perverse habit: the more current flows, the hotter and more conductive it gets, so even more current flows. Connected straight to a strong generator, it runs away into a short circuit, or blows out. Something in the circuit must limit the current — a ballast:

  • For direct current (DC): a resistor in series, such as a coil of thick iron wire. It works, but wastes power as heat.
  • For alternating current (AC): a choke — a coil of heavy wire on an iron core (see The Electromagnet) — which limits current with little waste. A The Transformer built with loosely coupled windings acts as its own choke.

The furnace operator also adjusts the arc length constantly by raising or lowering the electrode: longer arc, less current and more voltage; shorter arc, more current.

How much power

Job Energy needed, practical small furnace
Melting steel scrap and heating it to pouring heat 600–1,000 kWh per tonne (0.6–1 kWh per kg)
Calcium carbide about 3,000–4,000 kWh per tonne
Ferrosilicon (75% silicon) about 8,000–10,000 kWh per tonne
Silicon metal 12,000–15,000 kWh per tonne

A kilowatt-hour (kWh) is 1 kW for one hour. A furnace on a 30 kW supply melts roughly 30–50 kg of steel an hour once its lining is hot, but makes only about 2–3 kg of silicon an hour. A small furnace loses much of its heat through the walls, so very small furnaces do worse than the table.

What you need

Item For a 25–50 kg steel furnace
Power 20–50 kW, as 40–80 V AC or DC, at 300–800 A
Prime mover Water Turbines and Hydroelectric Power (for example 200 L/s falling 25 m gives about 35 kW) or a The Steam Engine of 40–80 horsepower
Generator A low-voltage dynamo or alternator wound with thick conductors, or a normal alternator plus a step-down The Transformer
Ballast Choke coil (AC) or iron-wire resistor grid (DC), adjustable
Conductors Copper bars of at least 5 cm² cross-section (for example 1 × 5 cm), or iron bars of 30 cm²; flexible stranded copper for the moving electrode
Electrodes Baked carbon rods 10–12 cm diameter, 1 m long; several spares
Shell Iron plate or a strapped brick box, 1 m across
Lining Burnt dolomite or magnesite (basic), or silica sand with a little clay (acid); firebrick backing. See Firebrick and Refractories
Ammeter Any current meter from Measuring Electricity used with a shunt
Additions Burnt lime, crushed iron ore or mill scale, coke or charcoal powder
Protective gear Very dark welding glass (see Welding), leather, wool clothing, dry wooden platform

Where to find it

  • Coke for electrodes comes from coal (see Coal and Coke). The best electrode carbon is hard, dense coke or the hard grey carbon that collects inside gas-works retorts. Pitch for binding comes from tar (see Tar, Pitch and Glue); coal-tar pitch is best. Wood charcoal makes weak, crumbly electrodes and is a poor substitute.
  • Graphite — natural flake graphite mixed into the electrode paste improves conductivity.
  • Lime, dolomite and quartz — see Lime, Steel in Quantity and Glass. Quartz for silicon must be pure white vein quartz or very pure quartz pebbles, in lumps 3–10 cm.
  • Scrap — any iron and steel. Sort out copper (it spoils steel), lead and galvanised (zinc-coated) iron.

Making carbon electrodes

1. Crush and sievehard coke: half grains1–5 mm, half fine flour 2. Mix hot80–85 coke to 15–20pitch, at about 150 °C 3. Ramthin layers into an irontube 10–12 cm across 4. Bakeburied in coke dust, slowlyto 1,000 °C; 1–2 weeks ram stir
Fig. 1 Making a baked carbon electrode. Crushed coke is mixed hot with pitch, rammed into an iron tube, and baked slowly in a kiln packed in coke dust so the pitch turns to carbon without burning.
  1. Crush and size the carbon. Crush hard coke and sieve it into two parts: about half as grains of 1–5 mm and half as fine powder like flour. The mixture of sizes packs densely. Add up to a fifth natural graphite if you have it.
  2. Mix hot. Heat coal-tar pitch to about 150 °C until it flows like thick syrup. Mix in the warm carbon at about 80–85 parts carbon to 15–20 parts pitch by weight, until every grain is coated and the paste is like stiff, warm dough.
  3. Ram. Pack the hot paste into an iron tube (10–12 cm inside, 1 m long) in thin layers, ramming each one hard with an iron rod. Push the "green" electrode out while it is still warm.
  4. Bake. Stand the electrodes in a The Kiln or a brick box, surrounded on all sides by coke dust or sand so air cannot reach them. Raise the heat very slowly — no more than 10–20 °C an hour at first — to about 1,000 °C (bright orange), hold it for a day, then cool slowly. The whole bake takes 1–2 weeks. The pitch gives off smoke and burning gas as it turns to carbon; hurrying cracks the rods.
  5. Test. A good electrode rings when tapped, is hard enough that a knife only scratches it, and is uniformly black-grey when broken, without cracks or soft centres.

A good baked carbon electrode carries about 5–7 amperes per square centimetre of cross-section. A 10 cm rod (78 cm²) carries about 400–550 A. Graphitised electrodes, made by heating baked rods to about 2,500 °C electrically, carry three times as much — a later refinement.

Tip Self-baking electrodes. For a submerged-arc furnace you can skip the kiln. Make a sheet-iron tube, fill it with the warm paste, and lower it into the furnace. The heat bakes the paste from the bottom as the tube descends, and the iron casing melts away into the charge. Weld or rivet on new tube sections at the top, and keep topping it up with paste. This is the Søderberg electrode.

Building the furnace

Carbon electrode10–12 cm thick; burnsaway, fed down slowly Firebrick roof Arc3–5 cm long, 40–80 V Slaglime, 3–5% of charge Bath of steel Tap hole and spout clay plug Rammed dolomite hearthon firebrick, in an iron shell Clamp and arm moves up and down Counterweighton a rope overa pulley Flexible cablefrom the choke Steel barsin the hearth carrycurrent back out Return lead
Fig. 2 A small single-phase arc furnace. Current comes down the top electrode, jumps the arc to the bath, and returns through steel bars set in the hearth. The operator raises and lowers the electrode with the counterweighted arm to keep the current steady.

The simplest furnace has one electrode from above and a conducting bottom.

  1. Shell. A round shell of iron plate or a square box of firebricks held by iron straps, about 1 m across and 70 cm high on the outside.
  2. Bottom electrode. Set 4–6 mild steel bars (3–4 cm thick) upright through the floor of the shell, so their tops are flush with the future hearth surface, and join their outer ends to a heavy copper or iron plate under the furnace. The return cable bolts to this plate. The steel bars melt at their tops, but the cold bottom ends stay solid and carry the current.
  3. Lining. Lay 10–15 cm of firebrick inside the shell. Ram the working hearth on top: a bowl 50–60 cm across and 20–25 cm deep, of crushed burnt dolomite or magnesite mixed with 10% hot tar, rammed in thin layers. The walls are firebrick, faced with the same rammed mix to the slag line.
  4. Tap hole and spout. Leave a hole 3–4 cm across at the lowest point of the bowl on one side, leading to a clay spout. Plug it with a clay-and-sand stopper.
  5. Working door. A door 25 × 20 cm opposite the spout, for adding lime and taking out slag.
  6. Roof. A removable domed lid of firebrick in an iron ring, with a central hole 3 cm wider than the electrode.
  7. Electrode arm. A horizontal iron arm holding a clamp of copper or thick iron round the electrode. The arm slides up and down a stout post, hung on a rope over a pulley with a counterweight, so one person can raise and lower it smoothly with a windlass. Insulate the arm from the post with dry hardwood blocks.
  8. Leads. Connect the electrode clamp with flexible stranded copper cable, so the arm can move; connect the hearth plate with solid bars. Keep both leads close together and parallel: big currents in loops waste power and heat nearby iron.
G A Turbine orsteam engine20–50 kW Generator40–80 V,300–800 A Switch Choke or resistorlimits the current; moreturns, less current Ammeterwatch it, move the electrode Furnacearc from electrode to bath,back out through the hearth return lead: keep it close to the supply lead
Fig. 3 The power circuit. Water or steam turns the generator; the choke or resistor limits the current; the operator watches the ammeter and moves the electrode to hold the current steady.

Step by step: melting steel scrap

  1. Dry and heat the lining. Burn a wood fire inside for a day before the first melt, then strike the arc on a bed of coke to bake the hearth for another hour or two.
  2. Charge dry scrap — heavy pieces at the bottom, light on top — until the furnace is full, about 25–50 kg for this size. Put a few lumps of coke in the middle under the electrode to start the arc. Nothing wet, oily, painted, or closed (no sealed pipes or tins).
  3. Strike the arc. With the power on, lower the electrode until it touches the charge, then raise it a few centimetres. Watch the ammeter; hold the current at your target (for example 400 A) by raising and lowering the arm.
  4. Bore down. The arc melts a hole straight down through the scrap. This is the noisiest, most unsteady stage: it crackles and roars and the current swings. Hold the current near the target with short, smooth movements.
  5. Melt down. Once a pool forms, the current becomes steady and the sound turns to a smooth hum. Push unmelted pieces from the walls into the pool with an iron bar through the door. Melt-down takes about 1–2 hours.
  6. Oxidising slag. Add burnt lime, about 3–5% of the charge weight, and a few handfuls of crushed iron ore or forge scale. The bath boils as carbon burns out, and phosphorus goes into the lime slag. Rake this slag off through the door after 20–30 minutes.
  7. Reducing slag. Add fresh lime with a little powdered coke or charcoal. This slag turns white and crumbly as it cools, and it pulls sulfur out of the steel.
  8. Adjust and deoxidise. Add ferromanganese and ferrosilicon (below) a few minutes before tapping, to remove oxygen and set the composition. Test the carbon by pouring a spoon sample and breaking it, as in Steel in Quantity.
  9. Check the heat. Dip a cold mild steel rod 1 cm thick into the bath for a few seconds: in pouring-hot steel (about 1,600 °C) the tip melts off almost at once. The steel looks white and runs off a spoon like water.
  10. Tap. Switch off, raise the electrode, knock out the tap-hole plug, and run the steel into a warmed, dry ladle or straight into moulds (see Metal Casting).

Ferroalloys, calcium carbide and silicon

Self-baking electrodepaste in a sheet-iron casing Contact clamp CO burns at the top Chargeore or quartz + coke,fed in as it sinks Hot craterround the buried tip,about 2,000 °C Molten productalloy or carbide, tappedevery 1–2 hours Tap hole Fresh charge Carbon hearthbaked paste or carbon blocks
Fig. 4 Submerged-arc smelting. The electrode is buried in the charge, so the heat stays down where the reactions happen. The product collects at the bottom and is tapped every hour or two; carbon monoxide burns at the surface.

For these, the furnace works differently. The electrode is pushed deep into the charge (submerged arc). The charge is fed continuously from the top as it sinks, and the molten product collects at the bottom and is tapped every 1–2 hours. Carbon monoxide escapes through the charge and burns in blue-yellow flames at the top.

Product Charge (by weight) Use
Ferrosilicon (45–75% silicon) Quartz lumps 100, coke or charcoal 50–60, iron turnings or scrap 20–50 Deoxidiser for steel; silicon steel for The Transformer cores
Ferromanganese (about 75% manganese) Manganese ore 100, coke 30–40, lime 10–15 Deoxidiser; manganese steels (Alloy and Stainless Steels)
Ferrochrome Chromite 100, coke 30–40, quartz 10–20 Stainless and chromium steels
Calcium carbide Burnt lime 60, coke 40, both in 1–5 cm lumps Acetylene — see Calcium Carbide and Acetylene
Silicon metal (about 98%) Pure quartz 100, charcoal 60–70, wood chips 30 Pure Silicon, aluminium alloys, chemistry

These ratios are starting points: adjust from how the furnace behaves. Too little carbon and a sticky slag builds up and the product comes out poor; too much carbon and the charge becomes too conductive, the electrode rides up, and the heat moves to the surface.

Calcium carbide comes out as a grey-black liquid at about 2,000 °C and is tapped into iron pans. When cold it is a grey stone that fizzes in water and smells of garlic (impurities in the acetylene). Break it and store it at once in sealed iron drums.

Silicon metal is the hardest of these: it needs the purest quartz, the purest charcoal, and steady high power. The wood chips keep the charge open so gas can escape. It solidifies into a shiny grey, brittle metal that looks like dark glass with a metallic lustre.

How to tell it worked

  • Steady arc. After bore-down, a smooth even hum and a steady ammeter needle mean the arc is burning on a liquid pool.
  • The pour. Hot steel runs from the spout like water and leaves no skull (frozen shell) in the ladle.
  • The metal. Steel from scrap should forge, bend and harden according to its carbon. Ferrosilicon is grey and brittle, and much lighter than iron. Ferromanganese is silvery and brittle.
  • The carbide test. A lump in water fizzes steadily and the gas burns with a bright, smoky flame.

Note Troubleshooting. Arc keeps going out → voltage too low, ballast too strong, or electrode raised too fast. Shorten the arc, reduce the ballast, or raise the voltage. Breakers trip or generator stalls on bore-down → too little ballast. Add resistance or choke turns until the worst short circuit is within the generator's limit. Electrodes break → cracked from fast baking, or the charge caves against them. Bake slower; charge carefully; keep the electrode clamp below the roof heat. Electrode clamp glows red → poor contact. Clean the contact surfaces and tighten. A loose clamp can melt. Hearth eaten through around the bottom bars → too little lining over the bars, or too hot too long. Rebuild with a thicker rammed bottom. Ferroalloy furnace "crusts" and gas blows out in jets → charge too fine or wet, or not enough wood chips. Poke the crust and open the charge with chips.

Dangers

Danger Arc light. The arc gives off intense ultraviolet light that burns the eyes and skin within seconds to minutes, like the worst sunburn. Eye burns ("arc eye") feel like sand under the lids 6–12 hours later and can damage sight. Never look at the arc without very dark welding glass (see Welding); cover all skin; put screens around the furnace so passers-by are protected.

Danger Electricity. The arc circuit's 40–100 V can kill through wet skin, and the generator or transformer side may be at much higher voltage. Stand on a dry wooden platform. Switch off before touching any electrode, clamp or cable. Never let two people handle the electrode arm at once.

Danger Water and molten metal. Wet scrap, a damp lining, a sealed pipe, or a cracked water-cooled part can explode into steam under the molten bath and throw steel across the shop. Dry everything; inspect every piece of scrap.

  • Carbon monoxide. Carbon electrodes and submerged-arc furnaces make a great deal of it. Work in a tall, well-ventilated shed, with the gas burning off at the top.
  • Fumes. Galvanised scrap gives white zinc oxide smoke that causes metal-fume fever (shivering and fever a few hours later). Remove zinc coatings and avoid lead.
  • Calcium carbide gives off flammable acetylene with any moisture. Keep it bone dry and away from flames until use.
  • Heat and burns. Wear wool and leather, never cloth that melts. Keep the area under the spout and ladle dry and sanded.
  • Loose connections in the heavy-current leads get red-hot and can start fires.

What this unlocks

With the arc furnace you can make high-quality steel from scrap and, using ferroalloys, all the Alloy and Stainless Steels — tool steels, spring steels and stainless steel. Calcium carbide gives acetylene for Welding and lighting (Calcium Carbide and Acetylene). Silicon leads to Pure Silicon and Semiconductors and the Transistor. Carbon electrodes are the same carbon anodes used to make Aluminium. Carborundum and graphite made in electric resistance furnaces give hard Abrasives and Grinding Stones and better electrodes and crucibles. The induction furnace in Electric Kilns and Furnaces melts steel without any electrode, heating the metal from inside.

How it was first done

Humphry Davy showed the brilliant arc between charcoal points at the Royal Institution in London around 1808–1810, using an enormous battery of some 2,000 plates. In 1878–1879 William Siemens melted a few kilograms of steel in an experimental arc furnace with a dynamo. In 1892 Henri Moissan in Paris used an arc furnace to reach well over 3,000 °C and made many carbides and other new compounds. In the same year Thomas Willson at Spray, North Carolina, while trying to make aluminium, produced calcium carbide in an arc furnace — and the acetylene industry began. Edward Acheson made carborundum in an electric resistance furnace in Pennsylvania in 1891, and later synthetic graphite at Niagara Falls. Paul Héroult, co-inventor of the aluminium process, built the first commercial arc furnace for steel at La Praz in the French Alps in 1900; Ernesto Stassano in Italy had built an indirect-arc furnace a few years before. In 1919 Carl Wilhelm Søderberg in Norway patented the self-baking electrode that made large ferroalloy and carbide furnaces practical.

Source: content/entries/metals/electric-arc-furnace.md