◆ Rebuild

Part 2 · Earth and Fire

Gem Cutting and Lapidary

How to saw, grind and polish stones harder than steel — agate, rock crystal, garnet, jasper — with nothing but soft metal, wood, water and graded grit. Domed cabochons and beads, flat faceted gems, and the useful hard parts of instruments — jewel bearings, agate pivot cups, balance knife-edges and polished windows.

Difficulty
●●●●●
Time
A day for a first polished cabochon; a week to build a lap and cut a faceted stone; jewel bearings take patient practice
Steps from zero
2 prerequisites →

You need first

Abrasives and Grinding Stones

This unlocks

Synthetic GemsJewellery, Beads and Medals
The full path from nothing — 2 steps before this one
  1. Stone Tools
  2. Abrasives and Grinding Stones
  3. Gem Cutting and Lapidary

Do them roughly in this order. See it on the tech tree →

Why it matters

Agate, rock crystal, jasper and garnet are harder than hardened steel. No file or chisel touches them. Yet with soft iron, copper, wood and a little grit, any patient person can saw them, shape them and polish them until they shine like glass. This craft is called lapidary (from the Latin for stone).

It is not only for ornaments, though beautiful stones have always been worth trading (Money, Trade and Record-keeping). Hard polished stone is a working material:

How it works

Hardness decides everything (Abrasives and Grinding Stones). Grit only cuts a stone softer than, or about as hard as, itself:

Stone Mohs hardness Cut by
Marble, serpentine, jet, amber 2–4 Sand, even sandstone; finish with tripoli
Obsidian, opal 5–6 Quartz sand; finish with tin oxide
Agate, jasper, rock crystal, flint (quartz family) 7 Quartz sand slowly; garnet or emery much faster
Garnet 6.5–7.5 Emery
Corundum (ruby, sapphire) 9 Only corundum itself (very slow) or diamond

The work always runs the same way: saw the rough stone into a slice, grind it to shape with coarse grit, smooth away the scratches with finer and finer grit, then polish with an extremely fine powder on a softer surface. The tool — a metal disc, a wooden wheel — never cuts the stone itself. It only carries the grit and presses it against the stone. That is why soft metals work best: grains of grit press into soft iron, copper, lead or tin and are held there like the teeth of a file.

Each step must remove all the scratches from the step before. A single deep scratch left from the coarse grit shows through a perfect polish.

What you need

Item Notes
Grit, graded Emery, garnet or crushed quartz, sorted by settling into at least four grades: coarse (0.1 mm), medium (0.05), fine (0.02), very fine (0.01) — Abrasives and Grinding Stones
Polishing powder Tin oxide (putty powder, from burning tin — Tin and Pewter), rouge, or tripoli
Slitting saw A frame saw with a soft iron blade, or a thin disc of soft iron or copper 15–20 cm across on a spindle
Lap A flat disc of cast iron, copper, lead or hard wood, 20–30 cm across, turning flat (horizontal) on a vertical spindle, driven by a treadle or a crank with a belt (The Lathe, Belts, Chains and Power Transmission)
Grinding wheel A sandstone wheel 20–30 cm across, running in water (Abrasives and Grinding Stones)
Polishing laps Wooden discs faced with leather, felt or a thin sheet of tin or lead
Dop sticks Hardwood dowels 10 cm long, 6–12 mm across
Dop wax Shellac and pine resin, melted together 1:1, with a spoon of brick dust per cup
Jamb peg A tapered wooden post drilled with holes, for faceting (see below)
Bow drill With copper or iron tube or wire bits (Drills and Boring)
Water pots, brushes, rags, a spirit or oil lamp For washing, and warming dop wax

Where to find it

  • Agate, chalcedony, jasper and carnelian: rounded nodules and pebbles in old lava flows and in the gravels of rivers and beaches below them. Translucent at thin edges, waxy, often banded. Chip a corner: it breaks like flint with smooth curved faces. See the materials list and Rocks and Minerals.
  • Rock crystal and amethyst: six-sided prisms in cavities in granite, pegmatite veins and geodes (Quartz Crystals and Frequency Control).
  • Garnet: dark red to brownish rounded crystals with twelve or more faces, the size of a pea or larger, studding mica schist; also as heavy red sand on beaches and in gold pans.
  • Corundum: rare. Barrel-shaped, six-sided crystals, grey, brown, blue or red, very heavy, in some marbles and pegmatites and in gem gravels with garnet; and as grains in emery. It scratches garnet and quartz easily.
  • Obsidian: black volcanic glass, easy to work and polish (Stone Tools).
  • Soft decorative stones: serpentine, marble, alabaster, jet, amber — cut with steel tools and sand, see Stone Carving.

Choosing rough: look for stone without cracks. Wet it — a wet surface shows how it will look polished — and hold it to a strong light to see inner fractures. A crack in rough will become a break in the finished stone.

The lap and the saw

The flat lap iron, copper or wood; wet grit on its face stone on dop Lap Spindle belt pulley below treadle and flywheel; 100–300 turns a minute The slitting saw soft iron or copper disc, 0.5–1 mm thick stone fed in gently Trough of grit and water
Fig. 1 The lapidary's bench. A flat metal lap turns horizontally on a vertical spindle, driven by a treadle and belt; wet grit on its face does the grinding. The slitting saw is a thin soft-iron disc whose edge, charged with grit and kept wet, slowly cuts a slice from the stone.

Building a lap

  1. Cast a disc of iron, copper or lead 20–30 cm across and 2–3 cm thick (Metal Casting), with a central hole.
  2. Mount it flat on top of a vertical spindle running in two bearings in a strong wooden frame (Bearings and Lubrication). Fix a pulley on the spindle below the table.
  3. Drive it by a belt from a treadle flywheel, a hand crank, or a water or animal wheel, at 100–300 turns a minute. For a hand drive, have a helper turn the crank.
  4. True the face: run it while holding a flat sandstone against it with water and coarse grit, until it is flat and evenly grey.
  5. Make several laps, one for each grade of grit, and never mix them. A wooden disc covered with leather or felt, or a disc of tin, is the polishing lap.

Sawing

  1. Frame saw (no machinery): stretch a strip of soft iron about 0.5 mm thick, or an iron wire, in a bow-saw frame. Wedge the stone in a block of wood or bed it in plaster. Keep a puddle of medium grit in water on the cut, and saw slowly back and forth with light pressure. The grit rolls under the blade and cuts; the blade wears too and must be replaced. Expect a centimetre of depth an hour in a 2–3 cm agate — less in quartz crystal, more in soft stone.
  2. Disc saw: a soft iron or copper disc 0.5–1 mm thick, 15–20 cm across, on a horizontal spindle like a grindstone, dipping into a trough of grit and water at the bottom. Feed the stone into the edge with steady light pressure, by hand or with a weighted arm. Faster than the frame saw. If you ever obtain diamond powder (Industrial Diamond and Hard Abrasives), press it into nicks hammered in the disc's edge with a hard roller: a "charged" disc cuts many times faster.
  3. Saw slices for cabochons 5–8 mm thick; for faceting, saw cubes or blocks of clean material.

Method 1: The cabochon

A cabochon is a stone with a flat back and a smooth domed top — the oldest and easiest gem shape, and the best for opaque and banded stones like agate and jasper.

1 Markdraw round atemplate2 Grindto the lineon the wheel3 Dopwarm wax ona wooden stick4 Domeroll it as yougrind, coarse→fine5 Polishtin oxide onleather or felt Making a cabochon from a slice of agate or jasper
Fig. 2 Making a cabochon. Mark the outline on a slice; grind to the line; fix the stone on a dop stick with warm wax; shape the dome by rolling it against the wheel; then smooth and polish with finer and finer grit.
  1. Mark the outline on the slice with a template: a thin brass sheet with an oval or round hole. Draw round the inside with a sharpened brass or aluminium wire — it leaves a silvery line that does not wash off.
  2. Trim close to the line with the saw, or by nibbling off corners with pliers, a little at a time.
  3. Grind the edge to the line on the sandstone wheel (wet) or the coarse lap, keeping the edge square to the back. Grind a small bevel all round the back edge so it does not chip.
  4. Dop it: warm the dop wax over a lamp until soft, press a blob onto the end of a dop stick, and shape it into a cone a little smaller than the stone. Warm the stone too (gently — cold stone on hot wax does not stick, and very hot stone cracks). Press the flat back of the stone onto the wax, centre it, and let it cool. The stick is now your handle.
  5. Shape the dome: hold the stick at an angle to the wheel or the coarse lap and roll it as you grind, working round and round the stone, lifting the angle gradually until you reach the top. Look often. Aim for an even curve with no flat spots; a dome as high as about a third of the stone's width looks well.
  6. Smooth: change to the medium lap with medium grit, and work the whole dome evenly until every coarse scratch has gone. Wash stone, stick and hands thoroughly. Then fine grit; then very fine. Check under a strong side light with a lens (Lenses); scratches show as bright lines.
  7. Polish: on the felt or leather lap, with a wet paste of tin oxide (best), rouge or tripoli, and light pressure. Keep the polishing lap just damp. The surface goes from grey satin to glassy in a few minutes when the smoothing has been done well. If it will not polish, you left scratches: go back one grade.
  8. Remove: put the stone and stick in cold water, or in a cold place, and give the stick a sharp twist; or warm the wax gently. Clean the wax off with alcohol (Ether, Acetone and Solvents).

Method 2: Faceting

Facets are small flat polished faces set at exact angles. In a clear stone like rock crystal, amethyst or garnet, light entering the top reflects off the angled facets at the back and comes out again through the top — the stone sparkles. To work, every facet must be cut at the right angle and the right position round the stone.

The jamb peg the hole chosen sets the facet's angle Peg rows of holes Dop stick 8-sided angle Flat lap grit, then polish Stick end turn one flat for the next facet mark Profile of a faceted quartz table crown 40° girdle pavilion 43° too flat a pavilion lets light leak out
Fig. 3 The jamb peg. The dop stick's end rests in one of many holes in a tapered wooden post beside the flat lap; the hole chosen sets the angle of the facet. Turning the stick in steps — marked by flats on an eight-sided stick — sets each facet's position round the stone.
  1. The jamb peg: a wooden post 20–30 cm tall beside the lap, with rows of holes drilled in its face at different heights. The far end of the dop stick rests in a hole while the stone touches the lap: a high hole gives a steep facet, a low one a shallow facet. Mark which hole gives which angle by trial with a protractor (Geometry and Trigonometry).
  2. The stick: plane the dop stick eight-sided. Each flat, turned to the top in turn, places the next facet one-eighth of the way round. For sixteen facets, cut a mark halfway between each flat.
  3. Shape the stone first by grinding it to a round outline (the girdle), then dop it with the top (table) side on the wax.
  4. Cut the pavilion (the pointed back): eight main facets meeting at a point, each at about 43° to the girdle for quartz. This angle matters: if the back is too flat, light leaks out through it and the stone looks dead. Cut each on the medium lap, then finish on fine, then polish on a tin or wooden lap with tin oxide — facet by facet, not all at once.
  5. Transfer: warm a second dop with wax, press it on the finished pavilion point with the two sticks held in a straight line (a V-groove block holds them aligned), let it cool, then warm and remove the first stick.
  6. Cut the crown (the top): eight main facets at about 40° to the girdle, then the flat table on top. Polish each.

A simple, handsome first design is the step cut: a rectangular stone with three rows of long facets stepping down on each side, top and bottom. Every facet is a straight cut, and the jamb peg is easy to set for it.

Method 3: Beads and drilling

  1. Grind a stone to a sphere by rolling it against the wheel in every direction, then smooth and polish it in a groove cut in a wooden lap.
  2. Drill with a bow drill (Drills and Boring) whose bit is a copper tube or a soft iron wire, fed with fine wet grit. The grit cuts; the bit carries it. A tube cuts a ring and leaves a core, which is faster than a solid bit.
  3. Drill halfway from each side, so the hole does not burst out and chip the far face. Mark the centres carefully on both sides.
  4. For agate, a 2 mm hole 1 cm deep takes about an hour of steady drilling.

Method 4: Hard parts for instruments

Pivot cups (cap jewels). For a compass needle or meter pointer that balances on a steel point: grind a small disc of agate or rock crystal 4–6 mm across, 2 mm thick. Drill a conical pit with a steel or copper point shaped to an angle a little wider than the pivot point (about 60–90°), charged with fine grit; then polish the pit with a wooden point and tin oxide (The Compass).

Hole jewels. For a turning shaft to pass through: a thin disc (1 mm) with a polished round hole. Without diamond, drilling a fine straight hole through hard stone is very slow: drill from both sides with a fine copper wire and the finest grit, then open and polish the hole with a hair-thin wire charged with oil and tin oxide, drawn through like a thread. Make garnet or agate jewels first; ruby and sapphire need diamond, or synthetic corundum grown for the purpose (Synthetic Gems).

Knife-edges for balances. Saw a small prism of agate 2–3 cm long, and grind two faces to meet at an angle of about 90° in a perfectly straight edge. Polish the faces; then very lightly round the edge itself with a few strokes on the polishing lap, so it does not chip. It rests on a flat, polished agate plane — a slip of agate ground and polished flat on both sides.

Flats and windows. For a perfectly flat face (a quartz window, a balance plane, a prism face), grind on a flat glass or iron plate by hand in figure-of-eight strokes, as for a crystal plate (Quartz Crystals and Frequency Control) or a lens (Lenses), and polish on pitch with rouge or tin oxide.

How to tell it worked

  • A good polish reflects a window sharply, with straight edges, and has no grey patches or fine scratches under a lens in a strong side light.
  • A cabochon's dome is smooth, with no flat spots when you roll it under a light.
  • A faceted stone looked at face-up sparkles across its whole table; a dark, "windowed" centre (you can read print through it) means the pavilion angles are too shallow.
  • A compass needle on an agate cup swings freely and settles slowly, and gives the same reading time after time.
  • An agate knife-edge balance returns to the same rest point after every swing.

Note Troubleshooting. Polish will not come up → scratches left from an earlier grade, or the polishing lap is contaminated. Go back a grade; wash everything; keep a separate covered lap for each grit. Fine scratches appear on a nearly polished stone → a coarse grain on the lap, from your hands or the air. Clean and cover the laps. Stone falls off the dop → stone or wax too cold when joined, or a greasy stone. Warm both, clean the stone with alcohol. Stone cracks while dopping → heated too fast. Warm slowly; some stones (opal, crystals with inclusions) need cold glue instead of wax. Edges chip → grind a small bevel on every edge before shaping; lighter pressure. Facets don't meet at a point → the stone was not centred on the dop, or the stick slipped round. Re-dop and re-cut.

Dangers

Warning Silica dust causes silicosis, an incurable lung disease, in lapidaries, stone-cutters and miners. Agate, jasper and rock crystal are pure silica. Work everything wet. Never grind or polish dry; wipe up dried slurry with a wet cloth, never sweep it; ventilate the workshop.

  • Lead laps shed lead into the slurry: wash hands before eating and keep children away from the bench (Lead). Prefer iron, copper, tin or wood.
  • Spinning wheels and saws catch fingers, sleeves and hair. A slipping stone can be thrown. Keep sleeves tight and stand to one side of a grindstone when starting it.
  • Eyes: chips fly from sawing and edge grinding. Wear eye protection.
  • Hot dop wax burns and sticks to skin; use a water bowl nearby to cool burns at once.

What this unlocks

The lapidary's skills of grinding and polishing hard materials to exact shapes are the same ones that make Lenses, The Telescope mirrors, Optical Glass and Achromatic Lenses prisms and quartz crystals. Jewel bearings make precise, long-lasting watches, compasses and meters possible, and agate edges make the fine balances of the chemist and the assayer.

Later: synthetic corundum (Synthetic Gems). Fine, pure aluminium oxide powder (Aluminium) sprinkled through an oxygen–hydrogen flame (Hydrogen, Oxygen and Gases) melts and builds up a single crystal of ruby or sapphire below it — the Verneuil process. It made jewel bearings cheap enough for every watch and meter, and gives an abrasive harder than emery in unlimited amounts.

How it was first done

People have drilled and polished stone beads for at least 40,000 years, and ground and polished stone axes since the Neolithic (Stone Tools). Egyptian craftsmen hollowed vases out of granite and hard stone with copper tube drills and sand more than 5,000 years ago. Mesopotamian seal-cutters engraved tiny cylinder seals in hard stone with bow drills and emery, and the bead-makers of the Indus valley drilled long carnelian beads with hard-stone drill bits about 4,500 years ago. Greek and Roman gem engravers carved intaglios and cameos in agate and onyx. Simple faceting appeared in Europe in the 14th and 15th centuries, and the more complex brilliant cuts in the 17th century. In 1704 Nicolas Fatio de Duillier and the watchmakers Peter and Jacob Debaufre patented the use of jewel bearings in watches in London; for two centuries jewels were cut by hand from natural ruby, sapphire and garnet. In 1902 Auguste Verneuil in Paris announced his flame-fusion method of growing synthetic ruby, and synthetic jewels soon replaced natural ones in instruments.