◆ Rebuild

Part 6 · Building

Plywood, Veneer and Boards

Wood splits along its grain and swells across it, and no tree gives a board a metre wide. Slice wood thin into veneer and glue the layers crosswise into plywood; press chips and sawdust into chipboard, or wood fibres into fibreboard and hardboard; glue planks face to face into laminated beams longer and stronger than any tree.

Difficulty
●●●●●
Time
A small hand-made plywood panel in a day plus a day in the press; a glulam beam in two days; a board factory is a whole industry
Steps from zero
11 prerequisites →

You need first

Basic WoodworkingGlues and Adhesives

This unlocks

—
The full path from nothing — 11 steps before this one
  1. Stone Tools
  2. Fire
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Basic Woodworking
  6. Hunting and Trapping
  7. Charcoal
  8. Pottery
  9. Hides and Leather
  10. Tar, Pitch and Glue
  11. Glues and Adhesives
  12. Plywood, Veneer and Boards

Do them roughly in this order. See it on the tech tree →

Why it matters

Solid wood has three faults that every carpenter fights:

  • It splits along the grain. A nail near the end of a board, a knot, or a dry summer opens a crack that runs the whole length.
  • It moves. Wood hardly changes in length as it dries or gets damp, but it shrinks 4–8% across its width from green to fully dry (Basic Woodworking). Even a seasoned 50 cm board changes by 5–10 mm between a wet winter and a dry summer, and it cups (curls across its face) as it does.
  • It comes only as wide and long as the tree. Wide boards need huge old trees, and long sound beams are rarer still.

Gluing wood in layers cures all three. Plywood — thin sheets glued with the grain of each crossing the next — does not split, barely moves, and is as wide as your press. Chipboard and fibreboard turn sawdust and waste wood into sheets. Glulam (glued laminated timber) builds beams and arches of any length and curve from ordinary planks.

These sheets and beams make cupboards, doors, floors, wall linings, boxes and crates, boat hulls, aircraft, concrete formwork and the roof arches of great halls (Furniture, Doors, Windows and Joinery, Boats and Sails, Gliders and Aeroplanes, Reinforced Concrete, Trusses and Frames).

How it works

Crossing the grain. Lay three thin sheets with the middle one's grain at right angles to the outer two. When the outer sheets try to shrink across their width, the middle sheet — which barely changes along its grain — holds them still, and the other way round. A crack starting in one layer stops at the glue line, because the next layer's fibres run across its path. Plywood moves only about 0.2–0.3% for the same change of damp that moves solid wood 4–8%.

Balance. The layers on each side of the centre must be mirror images — same wood, same thickness, same grain direction, same dampness. If one side is different, the panel warps like a bimetal strip. That is why plywood always has an odd number of plies (3, 5, 7…) with the outer two running the same way.

Spreading the faults. In a solid beam one big knot can break the whole thing. Glued from many thin layers, the knots and weak spots are scattered and no single one matters much. Glulam is therefore stronger than solid timber of the same wood and size, and the best layers can be put where the stress is highest.

The glue decides everything. A board is only as good as its glue in the conditions it meets (Glues and Adhesives):

Glue Water resistance Use for
Hide glue None: it lets go in damp Indoor furniture, veneering by hand
Casein glue Good in damp, not in soaking water Indoor and sheltered work, early aircraft plywood, the first glulam
Blood albumin glue (hot-pressed) Fairly good Early "water-resistant" plywood
Urea-formaldehyde resin Good indoors, slowly fails outdoors Most furniture plywood and chipboard
Phenol-formaldehyde resin Boil-proof Exterior and marine plywood, glulam outdoors
Solid board (end view) damp: flat, 50 cm widedries dry: 2–4 cm narrower, cupped,and split along the grain Plywood (layers pulled apart) facegrain along cross-bandgrain across coregrain along cross-bandgrain across backgrain along odd number of plies, mirror images about the core: it stays flat
Fig. 1 Why plywood is stable. A wide solid board cups and splits as it dries; in plywood each layer's grain crosses the next, so the layers hold each other flat and stop cracks at every glue line.

What you need

Item For Notes
Straight, knot-free logs Veneer Birch, poplar, alder, beech, pine, fir, spruce; 30 cm or more across
Planks 20–45 mm thick Glulam Dried to about 12% moisture, planed true
Sawdust, shavings, chips Chipboard Dry; screened by size
Wood, straw or cane fibre Fibreboard Pulped as for Paper
Glue All Hide glue, casein glue, or resins from Methanol and Formaldehyde (Resins: Phenolic, Polyester and Epoxy, Early Plastics)
A press All Iron screw clamps, a wedge press or a screw press; for factories a hydraulic press with steam-heated plates
Cauls Plywood Stiff hardwood bars 5 × 8 cm, planed with a slight hump (about 2 mm in 60 cm) so they press the middle first
A veneer lathe Peeled veneer A heavy The Lathe with a screw feed; water or steam power (The Waterwheel, The Steam Engine)

Where to find it

  • Veneer logs: the best "peeler" woods are straight, round, even-grained and fairly soft — birch (the classic plywood of Finland and Russia), poplar and aspen, alder, pine, Douglas fir, beech. Choose the lowest, branch-free 2–3 m of the trunk.
  • Waste wood for boards: sawmill slabs, edgings, sawdust and planer shavings (Sawmills and Lumber, Planers, Thicknessers and Woodworking Machines); thinnings and branch wood from coppice (Firewood and Coppicing); cereal straw and sugarcane waste (bagasse) for fibreboard.
  • Blood for albumin glue: from slaughter (Butchery and Meat), dried thin in the sun or a warm room to a dark red powder.

Veneer

Veneer is wood cut into sheets 0.5–4 mm thick. Thick veneer (2–4 mm) is for plywood cores and plain work; thin veneer (0.5–1 mm) of handsome wood is glued over cheap wood for fine furniture. Three ways to make it:

Rotary peeling (end view of the lathe) log turns chuck pressure bar squeezes the wood just ahead of the edge knife edge at centre height bevel 20–23°, as long as the log veneer ribbon, 1–3 mm knife carriage feeds in one veneer thickness per turn Sawn by hand saw kerf a thick plank, sawn along into 2–3 mm sheets; the saw cut wastes as much as it gives Sliced by a knife knife moves steamed block (flitch); 0.5–1 mm sheets kept in order to match the figure
Fig. 2 Three ways to cut veneer. Sawn from a plank by hand; sliced from a block by a knife; or peeled from a turning log by a long knife on a lathe, which gives a continuous ribbon.

Sawn veneer

The first method, and the only one with hand tools.

Plane one face of a dry, straight-grained plank 10–20 cm wide, gauge a line 3 mm in from it on both edges, stand the plank on edge in a vice and saw along the line with a fine frame saw (Files and Saws), from both edges toward the middle. Re-plane the plank and repeat; plane each sheet to an even 2–3 mm. Expect 4–6 sheets from 25 mm of plank: slow and wasteful, but it needs only hand tools.

Sliced veneer

Soften a squared block (flitch) by boiling or steaming it 1–3 days, clamp it down, and drive a long, very sharp knife (40–60 cm, bevelled about 20°) across it on a heavy sliding carriage, with a pressure bar just ahead of the edge, taking sheets 0.5–1 mm thick. Keep them in order: consecutive sheets match and can be laid in mirror-image (book-matched) patterns. This is how figured face veneers are cut; it needs a strong machine but makes no sawdust.

Rotary-peeled veneer

The plywood factory's method. A log is turned against a knife as long as the log, which peels off a continuous ribbon like unrolling paper from a roll.

  1. Cut logs ("peeler bolts") a little longer than the sheet: 1.3 m for small sheets, 2.6 m for a full 2.44 m sheet.
  2. Condition them: soak in hot water or steam at about 50–90 °C for 12–48 hours (birch and poplar near the low end, hardwoods higher). Cold, hard logs give rough veneer full of cracks.
  3. Mount the log between the lathe's spindle chucks (spiked plates driven into each end).
  4. Set the knife: bevel ground at 20–23°, its edge exactly level with the log's centre, tilted so the bevel barely clears the wood. A pressure bar (nosebar) presses the wood just ahead of the edge, squeezing the veneer by about a tenth of its thickness. Without it the veneer comes off with deep cracks on its inner side (lathe checks).
  5. Feed: the knife carriage moves in toward the centre by exactly one veneer thickness per turn, through gears and a feed screw like a screw-cutting The Lathe. 2 mm per turn gives 2 mm veneer.
  6. Peel until 8–15 cm of core is left (use it for fence posts, or chip it for chipboard, below). The first turns, until the log is round, give broken waste.
  7. Clip the ribbon into sheets with a long guillotine knife, cutting out splits and big knots.
  8. Dry quickly to 6–10% moisture, flat: on racks in a warm room with moving air, or between hot plates. Slow drying lets veneer cockle and mould.

A 40 cm birch log 2.6 m long gives about 0.15 m³ of veneer — some 30 m² of 4 mm plywood. Good veneer is even in thickness (within ±0.1 mm), smooth both sides, with few open checks when flexed inside-out.

Plywood

Method 1: Hand-made plywood

A first panel 60 × 90 cm, three plies, about 6–9 mm thick:

  1. Three sheets, equally dry: two faces of 2 mm veneer running lengthwise, a core of 2–4 mm running across. Join narrow sheets edge to edge with glued paper tape.
  2. Glue: casein (damp-resistant) or hot hide glue (indoor only), brushed thin and even on both sides of the core — about 150–250 g per square metre of glue line, no dry spots.
  3. Assemble at once (casein starts to gel in about 20 minutes), with paper or waxed cloth outside so squeeze-out does not glue it to the press.
  4. Press: lay the panel on a flat, stiff bed of planks; put a flat board on top, then cauls across it every 15 cm. Tighten iron screw clamps at both ends of each caul, middle cauls first, working outward so glue and air squeeze out to the edges. Aim for at least 1 kg on every square centimetre (0.1 MPa) — for this panel about 5–6 tonnes in all: 8–10 well-tightened iron clamps, or a wedge press (a strong frame of beams with pairs of wedges driven in hard).
  5. Leave it 6–12 hours (casein) or overnight (hide glue), then 2–3 days stacked flat under weights. Trim and scrape.

For thicker plywood add pairs of layers — 5 plies for 12–15 mm, 7 or 9 for 18–25 mm — each pair matched in wood and thickness.

Cabinetmakers lay face veneer on a ground with no press at all — hammer veneering: hot hide glue on both, then squeeze it out from the middle with a veneer hammer (a blunt blade 10 cm wide on a handle); the cooling glue grabs, and a warm iron re-melts any patch that has not stuck.

Method 2: The plywood factory

Industrial plywood follows the same steps on a large scale. Peeled veneers (1–3 mm) are graded (best for faces), glue-spread by rollers onto both sides of each core sheet, laid up, cold pre-pressed, then hot pressed in a hydraulic press with many openings (daylights) between steam-heated iron plates: 100–150 °C (about 115 °C for urea resin, 130–150 °C for phenolic), 1–1.8 MPa (10–18 kg per square cm), for about 5 minutes plus 1 minute per millimetre to the deepest glue line. Open the press slowly so steam does not blow the plies apart; then trim, sand and grade.

Standard sizes. Sheets 1.22 × 2.44 m (4 × 8 feet) became the world standard and suit house framing at 40–60 cm centres. Common thicknesses: 3, 4, 6, 9, 12, 15, 18 and 25 mm.

Bent plywood: thin veneers pressed between matching curved forms set into chair seats, hulls and fuselages.

Tell good plywood from bad

  • Tap it all over with a knuckle or a coin: a clear, solid sound everywhere. A dull, dead patch is a void or a lifted glue line.
  • Look at the edge: every ply continuous, no gaps or overlaps in the core, glue lines thin and even.
  • Flatness: a good panel lies flat on a flat floor. A warped one is unbalanced or was pressed at the wrong dampness.
  • Soak test: cut strips 2.5 × 10 cm and soak them a day in cold water, then dry. Interior plywood may soften but must not come apart. For exterior plywood, boil strips for 3–6 hours and try to pry the plies apart with a chisel: the wood should tear, not the glue line.
  • Nailing: drive nails 1 cm from the edge. Good plywood does not split.

Chipboard (particle board)

Chipboard is made of wood chips and sawdust glued under heat and pressure into a flat, dense sheet. It is cheap, flat and smooth, and uses wood that is otherwise waste. It is weaker than plywood, crumbles at the edges, and swells badly if it gets wet.

Method 1: Workshop board

Honest warning: hand-made chipboard is weak. It is still useful for drawer bottoms, panels behind cupboards, notice boards and pinboards.

  1. Sieve dry sawdust and shavings to 1–5 mm and dry them crisp.
  2. Mix about 1 part casein glue powder (or thick hide glue) to 4–6 parts wood by weight, until every particle is coated and the mix feels just damp.
  3. Form it in a wooden frame 2–3 cm deep on a waxed board, finest dust at top and bottom for smooth faces.
  4. Press as hard as your screw or wedge press can, to about a third of the loose depth. A day in the press, a week to dry.

Method 2: The factory

  1. Chip logs, slabs and edgings in a chipper; cut flakes 0.2–0.5 mm thick for the core and fine particles for the faces.
  2. Dry to just 2–4% moisture (the resin brings water with it).
  3. Blend: spray on urea-formaldehyde resin (about 8–12% of the chip weight on the faces, 6–8% in the core) with a hardener and about 1% melted wax to slow water uptake (Methanol and Formaldehyde).
  4. Form a loose mat: fine — coarse — fine. Pre-press it cold.
  5. Hot press at 180–220 °C and 2.5–3.5 MPa for a few minutes (roughly 10–20 seconds per millimetre of thickness). Cool, sand, cut.

Good chipboard weighs 600–750 kg/m³; the common thickness is 16–19 mm. Oriented strand board (OSB) uses long thin flakes laid in crossing layers, almost as strong as plywood, from small, fast-grown trees.

Tell good from bad: cut edge firm and tight, not crumbly; a screw driven into the face holds and needs force to pull out; a 5 cm square soaked a day in water swells by less than 15% of its thickness.

Fibreboard and hardboard

Fibreboard is wood broken into separate fibres and matted like very thick paper. Unpressed it is insulation board (softboard): light (200–400 kg/m³), 12–25 mm thick, for ceilings, linings and notice boards (Insulation and Keeping Buildings Warm or Cool). Pressed hot and hard it becomes hardboard: dense (900–1,100 kg/m³), 3–6 mm, smooth on one face, for drawer bottoms, panels and cupboard backs. Hardboard needs no glue: heat and pressure soften the wood's own lignin (the natural binder between fibres), which bonds them again.

  1. Make fibre. The workshop way is the papermaker's: boil wood chips, straw or cane waste with lye or lime, then beat them to a pulp (Paper). Factories steam chips at high pressure and grind them between ribbed discs, or let them burst from a steam gun.
  2. Form a wet mat on a wire screen from a thin slurry (1–2% fibre in water), as in papermaking, but 2–5 cm thick. Squeeze out water in a press.
  3. Insulation board: dry the mat slowly in a warm room or an oven at about 150–180 °C. Done.
  4. Hardboard: press the damp mat between hot iron plates at 180–220 °C and about 5 MPa (50 kg per square cm) for 5–10 minutes, with a wire screen under it so the steam escapes. The screen leaves its pattern on the back face.
  5. Re-dampen: a freshly pressed board is bone dry and will warp; hang it in damp air for a day or two.
  6. Tempered hardboard: dip in a drying oil such as linseed oil (Oils and Pressing) and bake at about 150–170 °C for several hours. It becomes harder and much more water-resistant.

Tell good hardboard: dense, hard to dent with a thumbnail, rings when you drop it flat, does not delaminate when the corner is bent. Soak a strip for a day: tempered board swells little; plain board swells and softens.

Glulam: glued laminated beams

A glulam beam is made of planks (laminations) glued face to face, with the grain all running along the beam. It can be any length, any depth and any curve.

Gluing up a straight beam (side view) light: the best, straightest laminations go in the top and bottom sixth of the depth red: scarf joints, staggered at least 60 cm apart in neighbouring layers screw clamps every 20–30 cm clamping bed Scarf joint 10–12 × the thicknessboth ends tapered to a long slope and glued:nearly as strong as unbroken wood Curved member over a form laminations bent over blocks;radius ≥ 150 × one lamination
Fig. 3 A glulam beam being glued up. Planks are joined end to end with long scarf or finger joints, staggered so no two are close together, then glued face to face and clamped on a bed. Curved members are clamped over a form.
  1. Laminations: planks 20–45 mm thick, dried to 8–15% moisture (no more than 5% difference between them) and planed flat on both faces within a day of gluing.
  2. End joints: make each lamination as long as the beam by joining planks end to end with a scarf joint — both ends cut to a long slope of 1 in 10 to 1 in 12 and glued. Later, factories use machine-cut finger joints.
  3. Grade: put the best, straightest, least knotty laminations in the outer sixth of the depth on each face (top and bottom), where bending stress is greatest. Stagger end joints so that joints in neighbouring layers are at least 60 cm apart.
  4. Glue: spread casein (dry, sheltered beams) or phenolic or resorcinol resin (outdoors) on both faces of each joint. Assemble the stack within the glue's working time.
  5. Clamp on a clamping bed — a row of strong iron brackets or posts every 30–40 cm on a level floor — with screw clamps every 20–30 cm, tightened from the middle outward, hard enough to squeeze a bead of glue from every line. Glulam needs high pressure: about 0.5–1 MPa.
  6. Cure: at least 24 hours in clamps above 15 °C; a week before loading.
  7. Plane the sides, which come out uneven, and round the edges.

Curves. For an arch or a curved rafter, bend the laminations over a form — blocks fixed to the floor along the curve — and clamp. Keep the radius at least about 150 times the lamination thickness (3 m for 20 mm laminations); tighter bends need thinner laminations. A laminated arch of this kind can roof a hall 20–40 m wide without columns.

Tell good glulam: glue lines thin and unbroken on both sides, the beam true after unclamping; a spare offcut split along a glue line with a wedge breaks in the wood, not the glue.

How to tell it worked

The tests are given with each product above. The general rule for every glued wood product: break a test piece on purpose. If it breaks through the wood with fibres torn from both faces, the glue and the pressing were good. If it breaks cleanly along a glue line, the glue was too thin, too old, the pressure too low, or the wood too damp or too dusty.

Note Troubleshooting. Plies come apart in patches → dry spots in the glue, glue gelled before pressing, or too little pressure in the middle. Spread more evenly, work faster, use humped cauls. Panel warps as it dries → unbalanced lay-up (different thickness, wood or dampness either side of the centre), or the panel was stored standing on edge unsupported. Stack it flat. Glue bleeds through thin face veneer → glue too thin or too much pressure for the open grain. Thicken it, use less. Veneer splits ahead of the knife → log too cold or dry, pressure bar not set. Condition longer, reset the bar. Chipboard crumbles → too little glue, too little pressure, or particles too wet when pressed. Hardboard blisters → steam trapped: mat too wet, no screen under it, or press opened too fast.

Dangers

Danger Formaldehyde. Urea- and phenol-formaldehyde resins give off formaldehyde as they cure and, for urea resin, for years afterwards. It irritates eyes and lungs, causes asthma, and causes cancer with long exposure. Mix and press in good ventilation, store new boards in an open shed for some weeks, and prefer casein and phenolic glues in homes and sleeping rooms (Methanol and Formaldehyde). Phenol itself burns skin badly (Early Plastics).

Danger Presses and lathes. A hydraulic or screw press closes with tonnes of force: hands out before it moves. Hot press plates at 150–220 °C burn instantly, and a press opened too fast can blow out steam and debris. A veneer lathe's knife is as long as the log and razor sharp; stop the lathe completely before clearing a jam, and never reach over a turning log.

  • Dust. Sanding plywood and chipboard makes very fine dust that inflames the lungs, and hardwood dust is linked to nose cancer. Wear a cloth mask, work outdoors or with moving air, and sweep up wet. Fine dust in a closed room can explode if a flame meets it.
  • Lifting: a full sheet of 18 mm plywood weighs about 35 kg and catches the wind like a sail; carry it on edge, two people outdoors. Fence hot log-conditioning vats.

What this unlocks

Plywood and boards make cheap, quick, flat furniture and cupboards (Cupboards, Drawers, Shelves and Desks), boxes and crates (Sacks, Boxes, Crates and Packaging), flush doors and floors (Doors, Hinges, Handles and Latches, Stairs, Floors and Interior Finishes), formwork for concrete (Reinforced Concrete), hulls (Boats and Sails), and light, strong frames for Gliders and Aeroplanes, kites and gliders. Plywood moulded over forms, and later layered with plastic resins and fibres, leads to the composite materials of modern aircraft and boats (Composites: Fibreglass, Carbon Fibre and Honeycomb, Glass Fibre and Glass Wool). Glulam arches let you roof wide halls without steel (Trusses and Frames).

How it was first done

Ancient Egyptian craftsmen glued thin wood layers crosswise: a coffin found at Saqqara, from about 2600 BC, appears to be made of six plies of wood pegged and glued. Veneering of fine woods onto plain ones was known in Egypt, Rome and China, and became a great art in 17th- and 18th-century European furniture. The Swedish engineer Immanuel Nobel (father of Alfred) is often credited with an early rotary veneer lathe in the 1840s, and plywood was made in quantity by the 1870s for chair seats, tea chests and pianos. The Portland Manufacturing Company in Oregon showed Douglas fir plywood at the 1905 Lewis and Clark Exposition, and the 4 × 8 foot sheet followed. Casein-glued plywood built many First World War aircraft, and waterproof phenolic glues arrived in the 1930s. William H. Mason invented hardboard ("Masonite") in Mississippi in 1924 with his steam gun, and Max Himmelheber in Germany patented chipboard in the 1930s; the first factories ran in the early 1940s. Otto Hetzer of Weimar patented glued laminated timber in 1906, and his arches roofed railway halls and exhibition buildings across Europe.