Iron and Brass Wire

Iron, steel and brass wire are drawn through a hard steel plate just as copper is, but they fight back harder, need cleaner metal, a better lubricant and careful annealing. This chapter covers preparing rod, the pickle–rust–lime coating that lets iron slide through the plate, water-powered draw benches and drawing drums, and what the wire is for — nails, pins, cards, heddles, fences, springs and cables.

Difficulty
●●●●●
Time
A week to make plates and a hand bench; a season to build a water-powered wire mill; a day to draw 50–200 m of iron wire by hand
Steps from zero
16 prerequisites →

You need first

SteelBlacksmithingCopper Wire

This unlocks

Troughs, Separators and Livestock GearEnvelopes, Stamps, Clips and Office SuppliesNeedles and PinsTungsten and Filament WireWire Rope and CableButtons, Buckles, Hooks and Zips
The full path from nothing — 16 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Bellows
  12. Iron (the Bloomery)
  13. Copper Smelting
  14. Blacksmithing
  15. Steel
  16. Copper Wire
  17. Iron and Brass Wire

Do them roughly in this order. See it on the tech tree →

Why it matters

Copper Wire carries electricity. Iron, steel and brass wire carry everything else. Iron wire is cheap and strong; steel wire is stronger than any rope; brass wire does not rust and is easy to bend into small parts. Together they give you:

The tools — draw plate, tongs, windlass bench — are those of Copper Wire. Read that chapter first. This one covers what changes when the metal is harder.

How it works

Drawing pulls a rod through a tapered hole slightly smaller than itself, so the metal flows thinner and longer (see Copper Wire). Three things are different with iron, steel and brass:

  1. They are stronger, so they need more pull. The force needed is roughly the metal's strength times the area coming out of the hole. Iron and brass need about twice the pull of copper of the same size; high-carbon steel three to four times.
  2. They work-harden fast. Each pass makes the wire harder and springier, until it splits or snaps. Iron and brass need annealing — heating to soften — after every three or four holes, steel sometimes after every two.
  3. Iron does not carry grease well. Bare iron rubbing on a steel plate tends to weld to it in tiny spots and tear. Iron wire-makers learned to give the rod a thin, rough skin — a trace of rust and a coat of lime — that holds the grease and keeps metal from touching metal. This coating is the secret of the trade.
Wire Pull to draw through a 3 mm hole Anneal after Annealing heat
Copper (for comparison) about 50–70 kg 3–4 holes Dull red, 500–600 °C; may be quenched
Brass (70 copper, 30 zinc) about 100 kg 2–3 holes Dull red, 550–650 °C; may be quenched
Soft iron about 100 kg 3–4 holes Cherry red, 700–800 °C; cool slowly in a closed pot
High-carbon steel about 200–250 kg 2–3 holes Just below cherry red, 680–720 °C, held an hour; cool very slowly

The finished wire's strength depends on the metal and on how much it was drawn since the last anneal ("hard-drawn" wire is drawn several holes after annealing and left hard):

Wire 2 mm thick Breaks at roughly
Soft (annealed) iron 95 kg
Hard-drawn iron 150–180 kg
Hard-drawn brass 150–190 kg
Hard-drawn high-carbon steel (spring wire) 450–650 kg

Strength goes with the area, so wire twice as thick holds four times as much. Use half these figures as a safe working load.

What you need

Item Notes
Rod to draw Iron, steel or brass, 5–8 mm thick; see "Making rod" below
Draw plates As in Copper Wire, but forged from your hardest Steel and tempered only to pale straw (about 220 °C). Keep one plate for iron and steel and one for brass and copper: hard metals wear holes larger
Draw bench with windlass As in Copper Wire, built heavier: the pull can reach 300–600 kg
Draw tongs Heavy, with sharp file-cut teeth in the jaws (Files and Saws)
Annealing pots Fired clay or iron pots with lids, big enough for a coil 30–40 cm across (Pottery, Firebrick and Refractories)
Pickle tubs Wooden or glazed tubs for sour liquor or weak acid
Lime Slaked lime from Lime
Grease Tallow, soap or beeswax (Soap, Beekeeping)
Charcoal For annealing and the forge (Charcoal)

Where to find it

There is nothing new to find: iron from Iron (the Bloomery) (or a The Blast Furnace and Cast Iron works and its finery), steel from Steel, brass from Zinc and Brass, lime from limestone (Lime), tallow from animal fat, charcoal from hardwood.

What matters is quality:

  • Iron must be clean. Slag streaks that do no harm in a hinge make wire snap. The best wire iron was always the softest, most thoroughly worked iron: fold and weld your bar iron several extra times (Blacksmithing), and break a test piece — a good bar breaks with a fine, grey, fibrous fracture and no black glassy streaks.
  • Steel for wire should be even in carbon. Crucible steel or well-folded shear steel is best (Steel).
  • Brass for wire should be 65–70% copper. "Yellow" brass with 60% copper is harder and cracks when drawn cold.

Making rod

  1. By hand. Forge bar iron into a long square rod, then round it in a swage — a block with a half-round groove, and a top tool with a matching groove — turning the rod between blows (Blacksmithing). Aim for 6–8 mm, even and free of folds. Tedious, but fine for a few kilograms.
  2. By slitting. Hot-roll iron into a thin flat strip, 6–8 mm thick, and slit it lengthwise into square rods with rotating cutters in a slitting mill (Sheet Metal and Rolling). Square rod draws fine: the first two or three holes round it.
  3. By grooved rolls. A rolling mill with rolls carrying round grooves of decreasing size turns a hot billet into rod directly (Sheet Metal and Rolling). This is how all wire rod has been made since the 1800s.
  4. Brass rod is cast in an open mould or a stone groove and hammered cold, annealing often, as for copper (Copper Wire, Metal Casting).

Point every rod: taper the last 5 cm by filing or hammering so it pokes through the next hole.

Step by step: preparing iron rod for the plate

This cleaning and coating cycle is repeated after every anneal. Skipping it is the commonest cause of torn wire and ruined plates.

1. Pickle sour liquor 12–24 h, or weak acid 15–30 min; scrub 2. Rust lightly hang wet 6–12 h until evenly stained brown 3. Lime dip in milk of lime, thin as cream; drip 4. Bake dry 100–200 °C for 1–3 h; no water may remain 5. Grease and draw through tallow or soap, then 2–4 holes 6. Anneal sealed pot, charcoal dust, cherry red; cool slowly
Fig. 1 The iron wire-maker's cycle. Scale is soaked off, a thin rust skin is grown, lime is put on and baked dry, and the coil is drawn with grease through two to four holes, then annealed and cleaned again.
  1. Pickle off the scale. Black scale from the forge or annealing is harder than the plate and will gouge it. Soak the coil in sour liquor — fermented bran water, sour whey or vinegar (Fermentation) — for 12–24 hours, or in weak sulfuric acid (about 1 part acid to 15–20 parts water, see Sulfuric Acid) for 15–30 minutes. Scale should come off with a scrub of sand. Rinse well.
  2. Rust it lightly ("sulling"). Hang the wet coil in the air, or sprinkle it with water a few times, for 6–12 hours, until it has a thin, even brown-yellow bloom of rust — not flaking, just stained. This soft skin carries grease into the plate.
  3. Lime it. Dip the coil in milk of lime (slaked lime stirred into water till it is like thin cream) and let it drip.
  4. Bake it dry. Hang it near the forge or in a warm oven, about 100–200 °C — too hot to hold, not glowing — for 1–3 hours. This drives off all water. Wet lime steams in the hole and tears the wire; and acid-pickled iron left unbaked can be brittle.
  5. Grease and draw. Pass the wire through a box of tallow, soap or a mixture of the two, just before the plate.

Brass and copper need only the pickle (vinegar with a spoon of salt per cup, as in Copper Wire), a rinse and grease. Do not rust them.

Method 1: Drawing by hand

Use the windlass bench and plate of Copper Wire.

  1. Push the pointed, coated rod through the first hole it will just enter and grip it with the toothed tongs.
  2. Wind steadily. Iron draws with a dry, squealing sound; a sudden scream or chatter means the grease has failed — stop, re-grease, and check the hole.
  3. Take two to four holes, then anneal. The plate's holes should step down about one-tenth in diameter each (the series in Copper Wire works for every metal).
  4. Anneal iron in a closed pot: coil the wire loosely, pack it in the pot with a handful of charcoal dust, lute the lid on with clay, and heat it in the forge or a kiln to cherry red (700–800 °C) for half an hour after the whole pot glows evenly. Then let it cool in the pot, slowly, ideally overnight in the dying fire. The charcoal eats the air in the pot, so the wire comes out grey and clean instead of thick with scale.
  5. Anneal brass at a dull red (550–650 °C) for 10 minutes and quench in water, or let it cool; either leaves it soft.
  6. Clean and coat again, and carry on.

With a hand windlass, two people can draw iron from 6 mm to 2 mm in a day, making perhaps 50–100 m of wire. Below 1.5 mm, one person can pull by hand, or wind onto a drum (Method 3).

Method 2: The water-powered draw bench

The medieval wire mills of Germany pulled rod in short strokes with water power: tongs grip, pull 30–40 cm, open, slide back, grip again. One mill did the work of many men, and it pulled harder and more evenly.

On the pullring slides out along the handles:jaws bite the wire pull On the returnring slides back to the joint:jaws open and slide back push Crankthrow 15–20 cm Pulling rod Plateon iron stop Grease box Rod coil 30–40 cm Waterwheel10–20 turns a minute Heavy timber bench, anchoredpull reaches several hundred kilograms
Fig. 2 A water-powered draw bench. A crank on the waterwheel shaft pulls the tongs away from the plate; on the pull the rope through their handles squeezes the jaws shut; on the return the jaws open and slide back for a fresh grip.
  1. Power. A crank on the shaft of a The Waterwheel (or one driven from it by Gears) turning about 10–20 times a minute, with a throw (crank radius) of 15–20 cm, giving a stroke of 30–40 cm. See Cranks, Cams and Linkages.
  2. The pulling rod. A long wooden rod, iron-strapped, runs from the crank pin to the tongs, sliding on a greased hardwood guide.
  3. Self-closing tongs. Their handles curve outward and pass through a loose iron ring (or a loop of chain) fastened to the pulling rod. When the rod pulls, the ring slides down the handles and squeezes the jaws shut — the harder the pull, the tighter the grip. When the rod pushes back, the ring slides up, the jaws spring open (a light spring or a cord to a weight helps), and the tongs slide back along the wire for the next bite.
  4. The plate sits against a heavy iron stop bolted to the bench frame, which must itself be built of heavy timbers and anchored: the pull is several hundred kilograms at every stroke.
  5. The worker sits facing the plate, feeds the wire, and keeps it greased. The rod coils off a reel on one side; the drawn wire is coiled on the other.

Each stroke leaves a tiny mark where the jaws bit. Fine wire is better drawn continuously, on a drum.

Method 3: The drawing drum (for 2 mm and below)

A drawing block is an upright wooden or iron drum 30–60 cm across, turned by a crank, a treadle and flywheel (Cranks, Cams and Linkages) or, better, through gears from a waterwheel. The point of the wire is pulled through the plate and fastened to the drum; as the drum turns, it pulls the wire through and coils it at the same time.

  • Turn it slowly at first: about 0.2–0.5 m per second at the surface of the drum. A 40 cm drum turning 15–25 times a minute is right.
  • The plate sits in a holder at the side of the drum, with a grease box in front of it.
  • A pawl and ratchet (Cranks, Cams and Linkages) stops the drum running back if the wire breaks.
  • Later wire mills set several drums in a row, the wire passing from one through the next plate onto the next drum, each drum turning a little faster than the last — the start of continuous wire drawing.

Steel wire

Steel wire is the strongest thing in this book for its weight. It is also the hardest to draw.

  1. Start soft. Before the first pass, and after each anneal, soften the steel fully: heat it in a closed pot to just below cherry red (680–720 °C), hold it there for an hour, and let it cool in the fire overnight. Steel quenched from red becomes glass-hard and will snap in the plate (Steel).
  2. Smaller steps. Draw only two or three holes between anneals; use plenty of grease and a good lime coat.
  3. The final draw. For spring and music wire, give the last four to six holes without annealing. The wire comes out hard and springy — far stronger than if it were hardened and tempered.
  4. Patenting (going further). Industrial steel wire is not annealed between draws but patented: heated bright red (about 900 °C) and then plunged into a bath of molten lead at about 450–550 °C, where it changes to a fine, tough structure that draws a long way without breaking. It makes the best piano wire and wire rope. The lead bath needs the care in Lead.

Spring wire. Coil hard-drawn steel wire round a rod while cold; let it spring open, then warm the coil to about 250–300 °C (a pale blue tint on a bright surface) for 15 minutes to relieve the strain. See Springs.

Brass wire and pins

Brass draws beautifully if it has enough copper and is annealed often. Two warnings:

  • Season cracking. Hard-drawn brass stored near ammonia — stables, urine, manure, some cleaning liquors — can split along its length weeks later. Gently heat finished brass parts to about 250–300 °C (until a drop of water dances on them) for half an hour to relieve the strain, and store them away from stables.
  • Lead in brass makes it easier to cut but ruins it for drawing. Keep wire brass lead-free.

Pins were the classic product. Draw brass wire to about 0.6–0.8 mm, straighten it by pulling it through a zigzag of pegs, cut it into lengths, point the ends on a fine grindstone (Abrasives and Grinding Stones), and fix a head — a tiny coil of wire squeezed on, or a head formed by striking the end in a die. Pins were then boiled with tin to whiten them (Tin and Pewter). The whole craft, and needle-making, is in Needles and Pins. Adam Smith counted eighteen separate jobs in an 18th-century pin workshop; ten workers dividing them made about 48,000 pins a day.

Uses, by size

Thickness Metal Use
3–5 mm Iron Wire nails, rivets, chain, fence wire, telegraph lines (about 4 mm), bucket handles, the wired edges of sheet-metal ware (Sheet Metal and Rolling)
2.5–4 mm Iron or soft steel, zinc-coated Fencing; barbed wire is two 2.5 mm strands twisted with short spiky barbs every 10–15 cm
1–3 mm Hard-drawn steel Springs, wire rope strands
1–2 mm Iron Binding, hooks, cages
0.4–1 mm Brass or iron Pins, heddles, sieves, jewellery, cloisonné (Enamel on Metal)
0.3–0.5 mm Hard steel or iron Card teeth, needles, fish hooks, instrument strings

Rust protection. Dip iron wire in molten zinc to galvanise it (Zinc and Brass), or in molten tin (Tin and Pewter), or coat it with hot tar or oil varnish.

Wire rope. Twist 6–19 wires into a strand, and 6 strands round a greased hemp core, all with the lay running the same way as in rope (Cordage and Rope). Wire rope is several times stronger than hemp rope of the same weight and does not rot. See Wire Rope and Cable for laying, splicing and safe loads.

How to tell it worked

  • Bend test. Iron wire should bend flat back on itself and straighten again without cracking. Hard-drawn wire springs back; soft wire stays bent.
  • Twist test. Clamp 20 cm of wire in a vice and twist the free end with pliers. Good iron wire takes many full turns and breaks with a clean, fibrous end. Wire that breaks after a few turns, or splits along its length, has slag or was over-drawn.
  • Even thickness. The 20-turns-round-a-stick test from Copper Wire.
  • Hang a weight from a sample and compare with the table above.
  • Brass should be bright yellow, without cracks after bending tight round its own thickness.

Note Troubleshooting. Iron wire tears, squeals and leaves bright smears in the hole → the coating failed. Rust it a little longer, lime it again, and bake it fully dry. Wire snaps at the plate every few metres → slag in the iron (look at the broken ends for black streaks), too big a step between holes, or it needed annealing. Wire splits lengthwise → slag streaks in the rod. Refold the bar iron or use better iron. Annealed iron comes out thick with black scale → air got into the pot. Lute the lid better and add charcoal dust. Steel wire snaps like glass after annealing → it was cooled too fast and hardened. Cool it in the pot, in the fire. Holes grow and the wire comes out thick → the plate is worn. Close the holes with a punch and re-ream, as in Copper Wire; harder steel plates last longer. Brass splits during drawing → too little copper, lead in it, or not annealed often enough. Finished brass cracks weeks later → season cracking; relieve the strain with gentle heat, and keep it away from ammonia.

Dangers

Danger Breaking wire under tension whips back with enough force to cut skin to the bone or take out an eye. Never stand in line with the wire or behind the tongs. Keep your face out of the line of the wire, and fit a board or a wooden hood over the plate. Stop the windlass, drum or water wheel before reaching in.

Danger Water-powered machinery cannot feel you. The crank and the drum keep going if a sleeve, hair or hand is caught. Fit a quick way to stop the wheel — a sluice gate that drops shut, or a clutch that disengages — within reach of the worker, and guard the crank.

  • Acid pickle burns skin and eyes; always add acid to water, never water to acid (Sulfuric Acid). Pickling iron in acid gives off hydrogen — no flames near the tub.
  • Lime burns eyes; rinse at once with lots of water (Lime).
  • Hot coils and annealing pots stay hot for hours and look cold.
  • Wire ends are needles; coils spring open. Wear eye protection when cutting and uncoiling.
  • Lead baths for patenting: see Lead.

What this unlocks

Cheap wire nails and rivets (Nails, Rivets and Wire Fasteners); card clothing for Textile Machinery; heddles for the The Loom; needles for Sewing, Needles and Thread and the The Sewing Machine; Springs for locks (Locks and Keys), clocks (The Mechanical Clock) and animal traps (Hunting and Trapping); fencing (Fences and Hedges); wire rope for Cranes and Lifting, Mining and Tunnelling and suspension bridges; telegraph lines (The Telegraph); spokes for the The Bicycle; strings for Musical Instruments; fine brass wire for cloisonné.

How it was first done

The earliest wire, from Egypt and Mesopotamia, was hammered or cut from sheet. Drawing through a plate spread in medieval Europe: the monk Theophilus described iron draw plates around 1120. In southern Germany — Nuremberg, Augsburg and the Altena district of Westphalia — wire-drawing was an organised trade by the 1300s, and by the mid-1400s water-powered draw benches were working there. England's first big wire works were set up at Tintern in the 1560s with German workers. Pins, carding combs and heddles were the main products for centuries.

The industrial age multiplied it. The German mining official Wilhelm Albert made the first practical wire rope in the Harz mines in 1834. In England, James Horsfall patented the lead-bath treatment of steel wire in 1854, giving very strong piano and rope wire. Iron and steel wire made the telegraph possible, and in the United States Joseph Glidden's barbed wire of 1874 fenced the prairies within a generation. The Roebling family's spun steel cables carried the Brooklyn Bridge, opened in 1883.