Part 2 · Earth and Fire
Charcoal
How to turn wood into charcoal by heating it with too little air to burn — in a pit, an earth-covered mound, or a sealed clay pot. Charcoal burns far hotter and cleaner than wood, and it is the fuel that makes metal possible.
- Difficulty
- ●●●●●
- Time
- A day to cut and stack; 1–5 days to burn; 1–2 days to cool
- Steps from zero
- 1 prerequisite →
You need first
FireThe full path from nothing — 1 step before this one
- Fire
- Charcoal
Do them roughly in this order. See it on the tech tree →
Why it matters
Wood is a poor fuel for serious heat. A third to a half of fresh wood's weight is water, and much of the rest leaves as smoke and flame before it gives its heat to anything. Charcoal is what is left when you drive all that out: nearly pure carbon, light, black and brittle. It burns with almost no smoke or flame, as a steady, intense glow. Blown with air, it reaches 1,100–1,300 °C — hot enough to melt copper and to smelt iron.
That is why charcoal matters so much:
- Metal. Every early metal — Copper Smelting, Bronze, Iron (the Bloomery), Steel — was smelted with charcoal. The charcoal is not just the fuel; its carbon pulls the oxygen out of the ore and leaves metal behind. A smith's forge burns it too (Blacksmithing).
- High heat for Glass, Glazes and crucible work.
- Clean cooking and heating without smoke, in a brazier or stove.
- Filtering — crushed charcoal cleans the taste and smell from drinking Finding and Purifying Water; specially treated charcoal does it far better (see Activated Charcoal).
- Black pigment for Ink and drawing.
- Chemistry — it is one of the ingredients of Black Powder (history), and is used in Soda Ash and Baking Soda making.
Charcoal is also light to carry: it weighs only about a fifth of the wood it came from.
How it works
Heat wood without enough air to let it burn, and it does not burn — it cooks. This is called pyrolysis (heat-splitting). The wood breaks down in stages:
| Wood temperature | What happens | Smoke you see |
|---|---|---|
| Up to 150–200 °C | Water boils out | Thick, white, wet (steam) |
| 200–280 °C | The wood starts to break apart; it browns | Heavy white-yellow, sharp-smelling |
| 280–400 °C | The main change: the wood gives off tar, vinegary acids and burnable gases. This step makes its own heat | Thick yellow-brown to grey, acrid, stings the eyes |
| 400–500 °C | Little but carbon is left | Thin, bluish, then almost clear |
What remains is charcoal: the black skeleton of the wood, 75–90% carbon, with the same shape and grain as the original piece.
The trick of every method is to heat the wood while starving it of air. A little of the wood (or some separate fuel) must burn to provide the starting heat. After that, the breakdown largely keeps itself going. If too much air gets in, your charcoal burns to ash. If too little heat reaches part of the pile, that part stays as half-cooked brown wood.
What you need
| Item | Amount | Notes |
|---|---|---|
| Wood | See each method | Hardwood gives dense, long-burning charcoal; softwood gives light charcoal that lights easily. Both work. |
| An axe or stone axe | 1 | See Stone Tools |
| Covering | Plenty | Leaves, dry grass, bracken or straw, then earth or turf |
| A shovel or digging stick | 1 | |
| Water | Several pots full | To put out flare-ups and opened charcoal |
| A long pole | 1 | For poking vent holes |
Wood choice. Use dead, dry wood, or green wood that has been cut and split and left to dry for at least two or three months. Dry wood makes more charcoal, faster. Best of all are dense hardwoods: oak, beech, hornbeam, hickory, maple, ash, birch, alder, eucalyptus and acacia. Pine and other conifers give a lighter, softer charcoal that is still good for forging. Cut wood into billets (short logs) 50–100 cm long. Split anything thicker than about 15 cm (a large hand's width). Pieces of similar size char evenly.
Tip Yields. Expect to get about one-fifth to one-quarter of the dry weight of your wood as charcoal from a pit or mound, and up to a third from a sealed retort. By volume, a pile shrinks by about half.
Method 1: The pit
Best for small batches — a few sacks — and for learning. No skill in stacking is needed.
- Dig a pit about 1 m wide and 1 m deep, with straight sides. Keep the earth piled beside it.
- Start a fire in the bottom with kindling and small sticks. Get it burning strongly.
- Add wood in layers. Put in a layer of billets. When the top of that layer is burning fiercely and the wood below has begun to blacken, add another layer. Keep doing this. The bottom layers sit in their own heat, under the burning layers, with little air: they turn to charcoal.
- Watch the smoke. It begins thick and white (steam), then turns yellowish-grey. Fill the pit to about 15 cm from the top.
- Seal it. When the last layer is burning well and the smoke has begun to thin and turn bluish, cover the pit quickly — first with a layer of green leaves, bark slabs or turf, grass side down, then with 15–20 cm of earth. Stamp it down. Seal every spot where smoke leaks out by throwing on more earth.
- Wait. Leave it for at least one full day, better two, until the earth on top is cold to the touch.
- Open carefully (see "Opening and storing" below).
A pit yields less than a mound — the first layers often burn partly to ash — but it is simple and forgiving.
Method 2: The earth mound (clamp)
For large amounts — enough to smelt metal — charcoal burners (colliers) have built mounds the same way for thousands of years. A mound 2 m across and 1.2 m high holds about 2 cubic metres of wood (around 800 kg if dry) and gives about 120–200 kg of charcoal.
Building the mound
- Choose the site. Flat, dry, sheltered from wind, with good earth nearby and no overhanging trees. Clear a circle 4 m across down to bare soil. An old charcoal site, with its black earth, is ideal.
- The chimney. In the centre, drive in three or four straight stakes in a ring about 25 cm across, standing about 1.5 m tall. This is the central chimney or flue. Fill its bottom 30 cm with dry kindling, dry grass and a few pieces of charcoal.
- Stack the wood. Stand billets on end, leaning slightly inward against the chimney, thick ends down, packed as tightly as you can. Fill gaps with smaller pieces — gaps let in air and burn to ash. Work outward in rings until the stack is about 2 m across. Lay a second, shorter tier on top and round the top off into a dome. Keep the chimney open all the way up.
- Cover it. Cover the whole stack with a layer of leaves, straw, bracken or grass 5–10 cm thick, so the earth cannot fall into the wood.
- Earth it over. Cover that with 10–15 cm of damp earth or turf (grass side down). Loamy, slightly damp soil that packs firmly is best. Leave the top of the chimney open. Around the bottom, leave 8–12 vent holes the size of a fist, evenly spaced.
Burning the mound
- Light it. Drop a shovel-full of glowing embers down the chimney onto the kindling. Push more dry tinder and small sticks down after it.
- Let it catch for 30–60 minutes, until the chimney is roaring and thick white smoke pours out. Then fill the chimney with short pieces of wood and cap it with a turf and earth.
- Steer the fire with vents. The fire now moves slowly from the top-centre, outward and downward. Smoke escapes from the base vents and through the earth. With a pole, poke small new vent holes in a ring about a third of the way down the mound. Watch the smoke from each:
- Thick white — the wood behind it is drying.
- Thick yellow-grey, acrid — that part is charring. Leave the vent open.
- Thin and blue, nearly clear — that part is done. Close the vent with earth and open a new ring of vents lower down.
- Work around the mound like this, ring by ring, until thin blue smoke comes from the vents at the very bottom. A 2 m mound takes 3–5 days and nights. Large traditional mounds of 10 m or more took two weeks.
- Guard it day and night. Two things go wrong:
- Flames break through the cover: throw damp earth on them at once. An open flame turns your charcoal to ash.
- Hollows form as wood shrinks inside, and the cover sinks or cracks. Fill hollows and cracks with earth as soon as you see them.
- Seal it. When the whole mound is giving thin blue smoke and has shrunk by about a third, close every vent and spread a fresh layer of earth over all of it. Leave it one to two days to cool and suffocate.
Warning Never stand or walk on a burning mound. The wood inside burns away and leaves hollows full of glowing charcoal under a thin crust of earth. Colliers have fallen through into them and been badly burned or killed. Use a ladder or board laid against the side to reach the top.
Method 3: The sealed pot (retort)
A retort is a sealed container heated from outside. The wood inside never meets air at all, so none of it burns to ash and none of the charcoal is wasted. It gives the cleanest, most even charcoal, and the highest yield — up to a third of the wood's weight.
- Make or choose a pot. Any sturdy, fired clay pot with a lid will do — 10–40 litres. You can make one for the purpose (see Pottery), with walls 1–1.5 cm thick and plenty of grog in the clay. Make one small hole, 6–10 mm across, in the lid or high in the side.
- Pack it tightly with dry wood pieces of even size: 2–5 cm thick, cut to fit.
- Seal the lid with a rope of clay mixed with sand pressed all round the join.
- Heat it. Set it on stones in a fire, or build a fire around it — the "two-container" idea: the sealed inner pot inside an outer ring of fire, which can be a wall of stones or a larger clay drum with an opening for fuel. Keep the fire going hard.
- Watch the hole. First steam comes out, then thick, yellowish smoke. Hold a burning stick to it: the smoke catches fire and burns as a jet of flame. (If you place the hole so this flame plays back into the fire, it adds a lot of heat and saves fuel.)
- Done when the jet of flame dies down and no more smoke comes out — usually 1–4 hours depending on size.
- Plug the hole with clay, pull the pot out of the fire, and let it cool completely before opening — at least a few hours.
Small version: the same works for making char cloth and charred tinder in a closed tin or pot (see Fire).
By-products. If the escaping smoke is led through a clay pipe into a cool pot, it condenses into a dark, sticky liquid: wood tar on the bottom and sour "wood vinegar" on top. See Tar, Pitch and Glue.
Opening and storing
Charcoal that is still hot inside will burst into flame the moment it meets air, even a day after the fire seems dead.
- Open the mound or pit from one side only, a section at a time, with a rake. Have water ready.
- Spread the charcoal out on bare ground. Watch it: any piece that glows or smokes, douse it or bury it in earth.
- Leave fresh charcoal in the open for a day before bagging or storing it. Fresh charcoal soaks up air and can heat itself and catch fire in a large heap.
- Store dry. Damp charcoal is hard to light and heavier to carry.
- Pick out the brown, half-burnt pieces (colliers call them "brands"). Keep them for the next burn.
How to tell it worked
- Colour: deep black right through, with a slight shine on broken faces. Brown or with a brown core = underdone.
- Sound: two good pieces knocked together ring with a high, almost metallic clink. Underdone pieces thud.
- Breaking: it snaps cleanly and crisply, showing the wood's grain.
- Weight: much lighter than the same piece of wood.
- Burning: it lights with a little effort, burns with no smoke, and only short blue flames, glowing bright orange when you blow on it.
Note Troubleshooting. Mostly ash, little charcoal → too much air; the cover was thin, cracked, or vents were left open too long. Earth more thickly and close vents as soon as smoke turns blue. Lots of brown, half-charred wood → not enough heat reached those parts, or the burn was stopped too early. Wood was too wet or too thick. Dry and split the wood more; keep the burn going until all vents give blue smoke. Mound will not stay lit after capping → not enough heat at the start; let the chimney burn longer before capping. Charcoal crumbles to small bits → normal for some woods (especially conifers); and from over-handling. Fine for forging.
Dangers
Danger Carbon monoxide. Burning charcoal makes large amounts of carbon monoxide, a gas with no smell or colour that kills in your sleep. Never burn charcoal, or keep a smouldering mound or brazier, inside a closed room, tent or shelter. Colliers who slept in huts beside their mounds made sure the huts were open and upwind. Headache, dizziness and confusion are the warning signs — get into fresh air at once.
- Falling into a mound — see the warning above.
- Burns and flare-ups when opening. Opened charcoal can flare up suddenly.
- Forest fire. A mound can burn for days. Clear the ground around it, keep water ready, and never leave it unwatched in wind.
- Self-heating. Fresh charcoal stored in a big heap can catch fire by itself. Cool it in the open for a day first.
- Smoke. The yellow smoke of charring wood is harsh and irritates eyes and lungs. Work upwind.
- Dust. Charcoal dust is dirty but not very poisonous; avoid breathing clouds of it. In a closed space, a dense cloud of fine dust can explode if lit.
What this unlocks
Charcoal is the fuel of the metal age: with Bellows, it smelts Copper Smelting, Lead and Iron (the Bloomery), and heats the forge for Blacksmithing and Steel. It fires Glass crucibles, and its by-products give Tar, Pitch and Glue. Crushed charcoal is a pigment for Ink, a filter for Finding and Purifying Water, and one of the three parts of Black Powder (history). Charcoal filaments made the first electric The Light Bulb.
How it was first done
Charcoal is as old as fire. People drew with it on cave walls at Chauvet in France more than 30,000 years ago. Deliberately made charcoal became essential when people began to smelt metal, from around 5000 BC in the Balkans and the Near East. For the next six thousand years, almost every piece of metal in the world was made with charcoal, and colliers lived in the forests tending their smoking mounds. So much wood was burnt that whole regions were cleared of forest, and managed woodland grew up to feed the colliers (see Firewood and Coppicing and Forestry and Tree Nurseries). In England, the shortage pushed Abraham Darby, in 1709, to smelt iron with coke — coal baked without air, just as wood is baked into charcoal (see Coal and Coke) — which helped start the Industrial Revolution.
Source: content/entries/earth/charcoal.md